A high-strength base film for composite current collector and preparation method thereof

Through the blending of modified PET resin and PP resin and electron beam radiation technology, a high-strength base film is formed, which solves the shortcomings of the existing base film for composite fluid collection in terms of mechanical mechanics, flame retardancy and thermal stability, and improves the Safety and performance of lithium batteries.

CN118772476BActive Publication Date: 2024-11-29扬州博恒新能源材料科技有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411280306.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-29
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

The existing base film for composite fluid collection has shortcomings in mechanical mechanical properties, flame retardancy, electrolyte resistance and thermal stability, which affects the safety and performance of lithium batteries.

Method used

The blending of modified PET resin and PP resin is used as the base film material, and the process of double screw extrusion, bidirectional stretching and electron beam radiation is combined with 1-allyl-3-vinyl imidazole chloride and 2, 4,6-trivinylboroxane and other components form high-strength base films, improving the mechanical and electrochemical properties of the base films.

Benefits of technology

It significantly improves the mechanical and mechanical properties, flame retardancy, electrolyte resistance and thermal stability of the base film, reduces contact resistance, extends service life, and is suitable for continuous large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high-strength base film for composite current collector and a preparation method thereof, and relates to the technical field of current collector for lithium battery, comprising the following raw materials by weight: 100 parts of modified PET resin, 20-25 parts of PP resin, 1-3 parts of compatibilizer, 3-5 parts of coupling agent, 0.8-1.5 parts of antioxidant, 0.7-1.2 parts of lubricant, 8-15 parts of fiber reinforced material, 10-15 parts of filler, 3-5 parts of 1-allyl-3-vinyl imidazole chloride, 1-3 parts of 2,4,6-trivinyl cycloboroxane; the modified PET resin is 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride co-modified PET resin. The base film has good mechanical properties, excellent flame retardancy, electrolyte tolerance and thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of current collectors for lithium batteries, and in particular to a high-strength base film for composite current collectors and a preparation method thereof. Background Art

[0002] The current collector is one of the indispensable components of lithium-ion batteries. It helps to reduce the internal resistance of lithium-ion batteries and improve the coulombic efficiency, cycle stability and rate performance of the battery. The main function of the current collector is to collect and output the current generated by the active material and input the electrode current to the active material. The current collector used in traditional lithium batteries is mainly a metal material current collector, which is heavy and is prone to internal short circuit when it is damaged by mechanical stress (especially extrusion, puncture, impact), thermal stress or electrical stress, thereby causing thermal runaway of the battery and leading to safety accidents. It can be seen that it is necessary to seek more effective methods to prepare new lithium battery current collectors that are light in weight, have little effect on battery energy density, are safer to use, and can achieve more effective electron transfer and mechanical support.

[0003] In order to improve the lightness and safety of the current collector, the concept of composite current collector was born. Composite current collectors generally adopt a sandwich structure of "metal conductive layer-polymer composite material-metal conductive layer". The polymer composite material is the base film for the composite current collector, which has insulation and flame retardant properties. The metal conductive layer is thin and will melt like a fuse in the event of a short circuit. It will melt quickly before thermal runaway. Battery damage is limited to the puncture site to form a "point break", effectively forming a "circuit-breaking effect", preventing continuous large current from causing battery overheating, and effectively solving safety problems. Therefore, the performance of the base film is the key to determining the quality of the composite current collector.

[0004] At present, the common composite current collector base films are PET base films and PP base films. These base films and metals have large contact resistance, which in turn increases the resistance of the battery, reduces the battery power, and affects the fast charging performance. In addition, they also have more or less technical defects such as insufficient flame retardancy, electrolyte tolerance, mechanical properties and thermal stability need to be further improved.

[0005] In order to solve the above problems, the Chinese invention patent with the authorization announcement number CN117261303B discloses a polypropylene film and its preparation method, composite current collector, electrode plate and application. The preparation method of the polypropylene film includes the following steps: melt extrusion treatment, casting treatment, biaxial stretching treatment and heat treatment of the raw materials in sequence to obtain a polypropylene film intermediate; in terms of mass percentage, the raw materials include 99%-99.95% polypropylene and 0.05%-1% additives, and the additives include polyacrylic acid-metal ion complexes; corona treatment of the polypropylene film intermediate to obtain a polypropylene film; the polypropylene film prepared by the preparation method of the application improves the storage stability of the surface adhesion performance of the polypropylene film, and realizes the stable preparation of the composite current collector with the polypropylene film as the base film. However, the polypropylene film as a base film for the current collector still has the defects of electrolyte tolerance and thermal stability, which still need to be further improved.

[0006] It can be seen that the art still needs a high-strength base film for a composite current collector having good mechanical properties, flame retardancy, electrolyte tolerance and thermal stability, and a preparation method thereof. Summary of the invention

[0007] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a high-strength base film for a composite current collector having good mechanical properties, flame retardancy, electrolyte tolerance and thermal stability and a preparation method thereof.

[0008] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a high-strength base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of modified PET resin, 20-25 parts of PP resin, 1-3 parts of compatibilizer, 3-5 parts of coupling agent, 0.8-1.5 parts of antioxidant, 0.7-1.2 parts of lubricant, 8-15 parts of fiber reinforcement material, 10-15 parts of filler, 3-5 parts of 1-allyl-3-vinyl imidazole chloride, and 1-3 parts of 2,4,6-trivinyl cycloboroxine; the modified PET resin is a PET resin co-modified by 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride and pentafluorobenzoyl chloride.

[0009] Preferably, the preparation method of the modified PET resin comprises the following steps: adding 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin and catalyst to an organic solvent, stirring and reacting for 1-3 hours in an ice-water bath, then heating to 90-110° C., continuing to stir and react for 4-6 hours, cooling to room temperature, rotary evaporating to remove the solvent, and then washing and vacuum drying in sequence to obtain the modified PET resin.

[0010] Preferably, the mass ratio of the 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin, catalyst and organic solvent is (6-8):(3-5):(70-90):(8-10):(250-350).

[0011] Preferably, the brand of the PET resin is PET CZ-333, which is provided by Jiangyin Xingye.

[0012] Preferably, the catalyst is anhydrous aluminum chloride.

[0013] Preferably, the organic solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide and N-methylpyrrolidone.

[0014] Preferably, the PP resin is PP F1002, provided by Yanshan Petrochemical.

[0015] Preferably, the compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is at least one of antioxidant 1010, antioxidant 168, and antioxidant 1076.

[0016] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.

[0017] Preferably, the lubricant is at least one of ethylene bisstearamide and butyl stearate.

[0018] Preferably, the fiber reinforcement material is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 3-6 μm and a length of 1-3 mm.

[0019] Preferably, the filler is a mixture of aluminum hydroxide flame retardant VK-LA50, aluminum powder and copper powder in a mass ratio of 1:(2-4):3; the particle size of the filler is 1200-1600 mesh.

[0020] Another object of the present invention is to provide a method for preparing the high-strength base film for the composite current collector, comprising the following steps:

[0021] Step S1, after uniformly mixing the modified PET resin, PP resin, compatibilizer, coupling agent, antioxidant, lubricant, fiber reinforcement material and filler according to weight parts, a composite material is obtained, and the composite material is sequentially extruded, cast and casted by a twin-screw extruder to form a sheet;

[0022] Step S2, stretching the sheet through a biaxial stretching process to form a base film;

[0023] Step S3, irradiating the base film under an electron beam, and then placing the irradiated base film in a solution containing a polar solvent, 1-allyl-3-vinyl imidazole chloride, 2,4,6-trivinyl cycloboroxine and ammonium ferrous sulfate, replacing the air with an inert gas, and then heating the base film for reaction. After taking it out, wash it with water for 3-6 times, and then dry it to obtain a high-strength base film for the composite current collector.

[0024] Preferably, the extrusion temperature of the twin-screw extruder in step S1 is 230-260° C., and the screw speed is 110-220 rpm.

[0025] Preferably, the biaxial stretching process in step S2 is specifically as follows: the stretching temperature is 115-120° C., the stretching rate is 110-80 mm / s, the heat setting temperature is 215-235° C., and the stretching ratio is 4:1.

[0026] Preferably, the polar solvent in step S3 is at least one of N,N-dimethylformamide, dimethyl sulfoxide, and N,N-dimethylacetamide; the radiation is carried out in an air atmosphere at room temperature, and is continuous electron beam radiation, with an absorbed dose of 50 to 350 kGy, a beam current of 10 to 90 mA, and a voltage of 180 to 430 kV.

[0027] Preferably, the mass ratio of the polar solvent, 1-allyl-3-vinylimidazolium chloride and ammonium ferrous sulfate in step S3 is (3-6):1:(0.03-0.05).

[0028] Preferably, the inert gas in step S3 is any one of nitrogen, helium, neon and argon.

[0029] Preferably, the reaction temperature of the heating reaction in step S3 is 60-75° C. and the reaction time is 4-8 h.

[0030] Due to the application of the above technical solution, the present invention has the following beneficial effects:

[0031] (1) The method for preparing a high-strength base film for a composite current collector disclosed in the present invention has a simple preparation process, convenient operation and control, high preparation efficiency and finished product qualification rate, low energy consumption, low dependence on equipment, is suitable for continuous large-scale production, and has a high value for promotion and application.

[0032] (2) The high-strength base film for composite current collector disclosed in the present invention comprises the following raw materials in parts by weight: 100 parts of modified PET resin, 20-25 parts of PP resin, 1-3 parts of compatibilizer, 3-5 parts of coupling agent, 0.8-1.5 parts of antioxidant, 0.7-1.2 parts of lubricant, 8-15 parts of fiber reinforcement material, 10-15 parts of filler, 3-5 parts of 1-allyl-3-vinyl imidazole chloride, and 1-3 parts of 2,4,6-trivinyl cycloboroxine; the modified PET resin is a PET resin co-modified by 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride and pentafluorobenzoyl chloride. Through the mutual coordination and joint action of the raw materials, the prepared base film has good mechanical properties, flame retardancy, electrolyte tolerance and thermal stability. Using modified PET resin and PP resin as the base material of the base film can combine the advantages of the two, and improve the compatibility of the two by modifying the PET resin; the phenyl-4-isoazole, pentafluorobenzene and ketone structure introduced after modification, under the multiple effects of electronic effect, steric effect and conjugation effect between the molecular structure of PET and PP, makes the mechanical properties of the manufactured base film product better, flame retardant and electrolyte tolerance better, and thermal stability better. On the other hand, after modification, the compatibility between the base film and the metal can be improved, thereby improving its performance stability when used in the base film, reducing contact resistance, and improving electrochemical performance.

[0033] (3) The high-strength base film for the composite current collector disclosed in the present invention forms an interpenetrating network structure on the surface of the film through electron beam radiation grafting, which can effectively improve the comprehensive performance and performance stability of the base film. At the same time, the introduced imidazole chloride and cycloboroxine structures cooperate with other groups and structures (phenyl-4-isoxazole, pentafluorobenzene, ketone structure, PET and PP structure) in the base film to further improve the mechanical properties, flame retardancy, electrolyte tolerance and thermal stability, enhance the adhesion between the base film and the metal, and reduce the contact resistance.

[0034] (4) The high-strength base film for the composite current collector disclosed in the present invention has excellent mechanical properties, flame retardancy, electrolyte tolerance and thermal stability, good surface adhesion performance and long service life through the reasonable selection of preparation process parameters and steps. DETAILED DESCRIPTION

[0035] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.

[0036] Embodiment 1, a high-strength base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of modified PET resin, 20 parts of PP resin, 1 part of compatibilizer, 3 parts of coupling agent, 0.8 parts of antioxidant, 0.7 parts of lubricant, 8 parts of fiber reinforcement material, 10 parts of filler, 3 parts of 1-allyl-3-vinyl imidazole chloride, and 1 part of 2,4,6-trivinyl cycloboroxine; the modified PET resin is a PET resin co-modified by 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride and pentafluorobenzoyl chloride.

[0037] The preparation method of the modified PET resin comprises the following steps: adding 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin and catalyst into an organic solvent, stirring and reacting for 1-3 hours in an ice-water bath, then heating to 90°C, continuing stirring and reacting for 4 hours, cooling to room temperature, removing the solvent by rotary evaporation, and then washing and vacuum drying in sequence to obtain the modified PET resin; the mass ratio of the 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin, catalyst and organic solvent is 6:3:70:8:250; the brand of the PET resin is PET CZ-333, which is provided by Jiangyin Xingye; the catalyst is anhydrous aluminum chloride; the organic solvent is dimethyl sulfoxide; the brand of the PP resin is PP F1002, which is provided by Yanshan Petrochemical. Through weight change calculation and elemental analysis, the grafting rate of 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride was 6.5%, and the grafting rate of pentafluorobenzoyl chloride was 2.9%.

[0038] The compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 1010; the coupling agent is the silane coupling agent KH550; the lubricant is ethylene bisstearamide; the fiber reinforcement material is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 3 μm and a length of 1 mm; the filler is a mixture of aluminum hydroxide flame retardant VK-LA50, aluminum powder and copper powder in a mass ratio of 1:2:3; the particle size of the filler is 1200 mesh.

[0039] A method for preparing the high-strength base film for the composite current collector comprises the following steps:

[0040] Step S1, after uniformly mixing the modified PET resin, PP resin, compatibilizer, coupling agent, antioxidant, lubricant, fiber reinforcement material and filler according to weight parts, a composite material is obtained, and the composite material is sequentially extruded, cast and casted by a twin-screw extruder to form a sheet;

[0041] Step S2, stretching the sheet through a biaxial stretching process to form a base film;

[0042] Step S3, irradiate the base film under an electron beam, then place the irradiated base film in a solution containing a polar solvent, 1-allyl-3-vinyl imidazole chloride, 2,4,6-trivinyl cycloboroxine and ammonium ferrous sulfate, replace the air with an inert gas, then heat and react, take it out and wash it with water 3-6 times, and then dry it to obtain a high-strength base film for a composite current collector. Through weight change calculation and elemental analysis, the grafting rate of 1-allyl-3-vinyl imidazole chloride is 1.9%, and the grafting rate of 2,4,6-trivinyl cycloboroxine is 0.5%.

[0043] The extrusion temperature of the twin-screw extruder in step S1 is 230°C and the screw speed is 110 rpm; the biaxial stretching process in step S2 is specifically: the stretching temperature is 115°C, the stretching rate is 110 mm / s, the heat setting temperature is 215°C, and the stretching ratio is 4:1.

[0044] The polar solvent in step S3 is N,N-dimethylformamide; the radiation is carried out in an air atmosphere at room temperature, and is continuous electron beam radiation with an absorbed dose of 50 kGy, a beam current of 10 mA, and a voltage of 180 kV.

[0045] The mass ratio of the polar solvent, 1-allyl-3-vinylimidazole chloride and ammonium ferrous sulfate in step S3 is 3:1:0.03; the inert gas in step S3 is nitrogen; the reaction temperature of the heating reaction in step S3 is 60° C. and the time is 4 hours.

[0046] Example 2, a high-strength base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of modified PET resin, 22 parts of PP resin, 1.5 parts of a compatibilizer, 3.5 parts of a coupling agent, 1 part of an antioxidant, 0.8 parts of a lubricant, 10 parts of a fiber-reinforced material, 12 parts of a filler, 3.5 parts of 1-allyl-3-vinyl imidazole chloride, and 1.5 parts of 2,4,6-trivinyl cycloboroxine; the modified PET resin is a PET resin co-modified with 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride and pentafluorobenzoyl chloride.

[0047] The preparation method of the modified PET resin comprises the following steps: adding 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin and a catalyst into an organic solvent, stirring and reacting for 1.5 hours in an ice-water bath, then heating to 95° C., continuing stirring and reacting for 4.5 hours, cooling to room temperature, rotary evaporating to remove the solvent, and then washing and vacuum drying in sequence to obtain the modified PET resin; the mass ratio of the 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin, catalyst and organic solvent is 6.5:3.5:75:8.5:270.

[0048] The PET resin is PET CZ-333, provided by Jiangyin Xingye; the catalyst is anhydrous aluminum chloride; the organic solvent is N,N-dimethylformamide; the PP resin is PP F1002, provided by Yanshan Petrochemical; the compatibilizer is compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 1076; the coupling agent is silane coupling agent KH560; the lubricant is butyl stearate; the fiber reinforcement material is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 4μm and a length of 1.5mm; the filler is a mixture of aluminum hydroxide flame retardant VK-LA50, aluminum powder and copper powder in a mass ratio of 1:2.5:3; the particle size of the filler is 1300 mesh.

[0049] A method for preparing the high-strength base film for the composite current collector comprises the following steps:

[0050] Step S1, after uniformly mixing the modified PET resin, PP resin, compatibilizer, coupling agent, antioxidant, lubricant, fiber reinforcement material and filler according to weight parts, a composite material is obtained, and the composite material is sequentially extruded, cast and casted by a twin-screw extruder to form a sheet;

[0051] Step S2, stretching the sheet through a biaxial stretching process to form a base film;

[0052] Step S3, irradiating the base film under an electron beam, and then placing the irradiated base film in a solution containing a polar solvent, 1-allyl-3-vinyl imidazole chloride, 2,4,6-trivinyl cycloboroxine and ammonium ferrous sulfate, replacing the air with an inert gas, and then heating the base film for reaction. After taking it out, wash it with water 4 times, and then dry it to obtain a high-strength base film for the composite current collector.

[0053] The extrusion temperature of the twin-screw extruder in step S1 is 240°C, and the screw speed is 140 rpm; the biaxial stretching process in step S2 is specifically: the stretching temperature is 116°C, the stretching rate is 100 mm / s, the heat setting temperature is 220°C, and the stretching ratio is 4:1.

[0054] The polar solvent in step S3 is dimethyl sulfoxide; the radiation is carried out in an air atmosphere at room temperature, is continuous electron beam radiation, has an absorbed dose of 150 kGy, a beam current of 30 mA, and a voltage of 230 kV; the mass ratio of the polar solvent, 1-allyl-3-vinyl imidazole chloride, and ammonium ferrous sulfate in step S3 is 4:1:0.035; the inert gas in step S3 is helium; the reaction temperature of the heating reaction in step S3 is 65°C, and the time is 5 hours.

[0055] Example 3, a high-strength base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of modified PET resin, 23 parts of PP resin, 2 parts of compatibilizer, 4 parts of coupling agent, 1.3 parts of antioxidant, 0.9 parts of lubricant, 12 parts of fiber reinforcement material, 13 parts of filler, 4 parts of 1-allyl-3-vinyl imidazole chloride, and 2 parts of 2,4,6-trivinyl cycloboroxine; the modified PET resin is a PET resin co-modified by 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride and pentafluorobenzoyl chloride.

[0056] The preparation method of the modified PET resin comprises the following steps: adding 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin and catalyst into an organic solvent, stirring and reacting for 2 hours in an ice-water bath, then heating to 100° C., continuing stirring and reacting for 5 hours, cooling to room temperature, removing the solvent by rotary evaporation, and then washing and vacuum drying in sequence to obtain the modified PET resin; the mass ratio of the 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin, catalyst and organic solvent is 7:4:80:9:300; the brand of the PET resin is PET CZ-333, which is provided by Jiangyin Xingye; the catalyst is anhydrous aluminum chloride; and the organic solvent is N-methylpyrrolidone.

[0057] The PP resin is of the brand PP F1002, provided by Yanshan Petrochemical; the compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 1076; the coupling agent is silane coupling agent KH570; the lubricant is ethylene bisstearamide; the fiber reinforcement material is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 4.5 μm and a length of 2 mm; the filler is a mixture of aluminum hydroxide flame retardant VK-LA50, aluminum powder and copper powder in a mass ratio of 1:3:3; the particle size of the filler is 1400 mesh.

[0058] A method for preparing the high-strength base film for the composite current collector comprises the following steps:

[0059] Step S1, after uniformly mixing the modified PET resin, PP resin, compatibilizer, coupling agent, antioxidant, lubricant, fiber reinforcement material and filler according to weight parts, a composite material is obtained, and the composite material is sequentially extruded, cast and casted by a twin-screw extruder to form a sheet;

[0060] Step S2, stretching the sheet through a biaxial stretching process to form a base film;

[0061] Step S3, irradiating the base film under an electron beam, and then placing the irradiated base film in a solution containing a polar solvent, 1-allyl-3-vinyl imidazole chloride, 2,4,6-trivinyl cycloboroxine and ammonium ferrous sulfate, replacing the air with an inert gas, and then heating the base film for reaction. After taking it out, wash it with water 5 times, and then dry it to obtain a high-strength base film for the composite current collector.

[0062] The extrusion temperature of the twin-screw extruder in step S1 is 245°C, and the screw speed is 180 rpm; the biaxial stretching process in step S2 is specifically: the stretching temperature is 117°C, the stretching rate is 95 mm / s, the heat setting temperature is 225°C, and the stretching ratio is 4:1.

[0063] The polar solvent described in step S3 is N,N-dimethylacetamide; the radiation is carried out in an air atmosphere at room temperature, is continuous electron beam radiation, has an absorbed dose of 250 kGy, a beam current of 60 mA, and a voltage of 330 kV; the mass ratio of the polar solvent, 1-allyl-3-vinyl imidazole chloride, and ammonium ferrous sulfate described in step S3 is 4.5:1:0.04; the inert gas described in step S3 is neon; the reaction temperature of the heating reaction in step S3 is 69°C, and the time is 6 hours.

[0064] Example 4, a high-strength base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of modified PET resin, 24 parts of PP resin, 2.5 parts of compatibilizer, 4.5 parts of coupling agent, 1.4 parts of antioxidant, 1.1 parts of lubricant, 14 parts of fiber reinforcement material, 14 parts of filler, 4.5 parts of 1-allyl-3-vinyl imidazole chloride, and 2.5 parts of 2,4,6-trivinyl cycloboroxine; the modified PET resin is a PET resin co-modified by 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride and pentafluorobenzoyl chloride.

[0065] The preparation method of the modified PET resin comprises the following steps: adding 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin and a catalyst into an organic solvent, stirring and reacting for 2.5 hours in an ice-water bath, then heating to 105° C., continuing stirring and reacting for 5.5 hours, cooling to room temperature, removing the solvent by rotary evaporation, and then washing and vacuum drying in sequence to obtain the modified PET resin; the mass ratio of the 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin, catalyst and organic solvent is 7.5:4.5:85:9.5:340; the brand of the PET resin is PET CZ-333, which is provided by Jiangyin Xingye; the catalyst is anhydrous aluminum chloride; and the organic solvent is a mixture of dimethyl sulfoxide, N,N-dimethylformamide and N-methylpyrrolidone in a mass ratio of 1:2:3.

[0066] The PP resin is PP F1002, provided by Yanshan Petrochemical; the compatibilizer is CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is a mixture of antioxidant 1010, antioxidant 168, and antioxidant 1076 in a mass ratio of 1:2:3; the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570 in a mass ratio of 1:1:2; the lubricant is a mixture of ethylene bisstearamide and butyl stearate in a mass ratio of 3:5; the fiber reinforcement material is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 5 μm and a length of 2.5 mm; the filler is a mixture of aluminum hydroxide flame retardant VK-LA50, aluminum powder, and copper powder in a mass ratio of 1:3.5:3; the particle size of the filler is 1500 mesh.

[0067] A method for preparing the high-strength base film for the composite current collector comprises the following steps:

[0068] Step S1, after uniformly mixing the modified PET resin, PP resin, compatibilizer, coupling agent, antioxidant, lubricant, fiber reinforcement material and filler according to weight parts, a composite material is obtained, and the composite material is sequentially extruded, cast and casted by a twin-screw extruder to form a sheet;

[0069] Step S2, stretching the sheet through a biaxial stretching process to form a base film;

[0070] Step S3, irradiating the base film under an electron beam, and then placing the irradiated base film in a solution containing a polar solvent, 1-allyl-3-vinyl imidazole chloride, 2,4,6-trivinyl cycloboroxine and ammonium ferrous sulfate, replacing the air with an inert gas, and then heating the base film for reaction. After taking it out, wash it with water 6 times, and then dry it to obtain a high-strength base film for the composite current collector.

[0071] The extrusion temperature of the twin-screw extruder in step S1 is 255°C, and the screw speed is 210 rpm; the biaxial stretching process in step S2 is specifically: the stretching temperature is 118°C, the stretching rate is 85 mm / s, the heat setting temperature is 233°C, and the stretching ratio is 4:1.

[0072] The polar solvent in step S3 is a mixture of N,N-dimethylformamide, dimethyl sulfoxide, and N,N-dimethylacetamide in a mass ratio of 1:1:1; the radiation is carried out in an air atmosphere at room temperature, is continuous electron beam radiation, has an absorbed dose of 340 kGy, a beam current of 80 mA, and a voltage of 420 kV.

[0073] The mass ratio of the polar solvent, 1-allyl-3-vinylimidazolium chloride and ammonium ferrous sulfate in step S3 is 5.5:1:0.045; the inert gas in step S3 is argon; the reaction temperature of the heating reaction in step S3 is 73° C. and the reaction time is 7.5 h.

[0074] Example 5, a high-strength base film for a composite current collector, comprising the following raw materials in parts by weight: 100 parts of modified PET resin, 25 parts of PP resin, 3 parts of compatibilizer, 5 parts of coupling agent, 1.5 parts of antioxidant, 1.2 parts of lubricant, 15 parts of fiber reinforcement material, 15 parts of filler, 5 parts of 1-allyl-3-vinyl imidazole chloride, and 3 parts of 2,4,6-trivinyl cycloboroxine; the modified PET resin is a PET resin co-modified by 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride and pentafluorobenzoyl chloride.

[0075] The preparation method of the modified PET resin comprises the following steps: adding 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin and catalyst into an organic solvent, stirring and reacting for 3 hours in an ice-water bath, then heating to 110° C., continuing stirring and reacting for 6 hours, cooling to room temperature, removing the solvent by rotary evaporation, and then washing and vacuum drying in sequence to obtain the modified PET resin; the mass ratio of the 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin, catalyst and organic solvent is 8:5:90:10:350; the brand of the PET resin is PET CZ-333, which is provided by Jiangyin Xingye; the catalyst is anhydrous aluminum chloride; and the organic solvent is N,N-dimethylformamide.

[0076] The PP resin is of the brand PP F1002, provided by Yanshan Petrochemical; the compatibilizer is the compatibilizer CMG9801 provided by Jiayirong Polymer (Shanghai) Co., Ltd.; the antioxidant is antioxidant 1010; the coupling agent is silane coupling agent KH550; the lubricant is ethylene bisstearamide; the fiber reinforcement material is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 6 μm and a length of 3 mm; the filler is a mixture of aluminum hydroxide flame retardant VK-LA50, aluminum powder and copper powder in a mass ratio of 1:4:3; the particle size of the filler is 1600 mesh.

[0077] A method for preparing the high-strength base film for the composite current collector comprises the following steps:

[0078] Step S1, after uniformly mixing the modified PET resin, PP resin, compatibilizer, coupling agent, antioxidant, lubricant, fiber reinforcement material and filler according to weight parts, a composite material is obtained, and the composite material is sequentially extruded, cast and casted by a twin-screw extruder to form a sheet;

[0079] Step S2, stretching the sheet through a biaxial stretching process to form a base film;

[0080] Step S3, irradiating the base film under an electron beam, and then placing the irradiated base film in a solution containing a polar solvent, 1-allyl-3-vinyl imidazole chloride, 2,4,6-trivinyl cycloboroxine and ammonium ferrous sulfate, replacing the air with an inert gas, and then heating the base film for reaction. After taking it out, wash it with water 6 times, and then dry it to obtain a high-strength base film for the composite current collector.

[0081] The extrusion temperature of the twin-screw extruder in step S1 is 260°C and the screw speed is 220 rpm; the biaxial stretching process in step S2 is specifically: the stretching temperature is 120°C, the stretching rate is 80 mm / s, the heat setting temperature is 235°C, and the stretching ratio is 4:1.

[0082] The polar solvent described in step S3 is N,N-dimethylformamide; the radiation is carried out in an air atmosphere at room temperature, is continuous electron beam radiation, has an absorbed dose of 350 kGy, a beam current of 90 mA, and a voltage of 430 kV; the mass ratio of the polar solvent, 1-allyl-3-vinyl imidazole chloride, and ammonium ferrous sulfate described in step S3 is 6:1:0.05; the inert gas described in step S3 is nitrogen; the reaction temperature of the heating reaction in step S3 is 75°C, and the time is 8 hours.

[0083] Comparative Example 1, a high-strength base film for a composite current collector, is basically the same as Example 1, except that PET resin is used instead of modified PET resin.

[0084] Comparative Example 2, a high-strength base film for a composite current collector, is substantially the same as Example 1, except that 1-allyl-3-vinylimidazolium chloride and 2,4,6-trivinyl cycloboroxine are not added.

[0085] In order to further illustrate the beneficial technical effects of the high-strength base film for composite current collectors involved in each embodiment of the present invention, relevant performance tests were performed on the high-strength base film for composite current collectors involved in Examples 1-5 and Comparative Examples 1-2, and the film thickness of the test sample was 6 microns; the test method is as follows:

[0086] (1) Tensile properties: Tensile strength test is carried out according to GB / T 1040.1-2018.

[0087] (2) Heat aging resistance: The high-strength base film products for each composite current collector were placed in hot air at 85°C for artificial accelerated aging for 168 hours. After cooling to room temperature, the tensile strength was measured again. The heat aging resistance was measured by the retention rate of the tensile strength. The larger the value, the better the heat aging resistance.

[0088] (3) Flame retardancy: tested according to UL94 standard.

[0089] (4) Electrolyte tolerance: The composite current collector prepared in each example was cut into samples of 20 cm × 20 cm using a high-strength base film, and the circumference of the sample was recorded as C. 1 Then, place it in an electrolyte at 65℃ for 48h, and record the circumference of the sample after immersion as C. 2 The swelling degree SD of the sample is calculated according to the following formula: SD = (C 2 -C 1 ) / C 1 × 100%, the electrolyte is a mixture of ethylene carbonate, diethyl carbonate and methyl ethyl carbonate in a mass ratio of 1:2:1; the smaller the swelling degree, the better the tolerance of the electrolyte.

[0090] (5) Thermal stability: The thermal shrinkage rate of the base film involved in each example was tested with reference to ASTM D 1204. The smaller the value, the higher the thermal stability. The test is the thermal shrinkage rate of the film after the film is placed at 150°C for 30 minutes.

[0091]

[0092] As can be seen from Table 1, the high-strength base film for the composite current collector involved in each embodiment of the present invention has better mechanical properties, more excellent heat aging resistance, flame retardancy, electrolyte tolerance and thermal stability than the comparative example products, and the combined use of modified PET resin, 1-allyl-3-vinylimidazolium chloride and 2,4,6-trivinyl cycloboroxine is beneficial to improving the above properties.

[0093] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. All equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-strength base film for a composite current collector, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of modified PET resin, 20-25 parts of PP resin, 1-3 parts of compatibilizer, 3-5 parts of coupling agent, 0.8-1.5 parts of antioxidant, 0.7-1.2 parts of lubricant, 8-15 parts of fiber reinforcement material, 10-15 parts of filler, 3-5 parts of 1-allyl-3-vinyl imidazole chloride, and 1-3 parts of 2,4,6-trivinyl cycloboroxine; the modified PET resin is a PET resin co-modified by 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride and pentafluorobenzoyl chloride; The method for preparing the high-strength base film for the composite current collector comprises the following steps: Step S1, after uniformly mixing the modified PET resin, PP resin, compatibilizer, coupling agent, antioxidant, lubricant, fiber reinforcement material and filler according to weight parts, a composite material is obtained, and the composite material is sequentially extruded, cast and casted by a twin-screw extruder to form a sheet; Step S2, stretching the sheet through a biaxial stretching process to form a base film; Step S3, irradiating the base film under an electron beam, and then placing the irradiated base film in a solution containing a polar solvent, 1-allyl-3-vinyl imidazole chloride, 2,4,6-trivinyl boroxine and ammonium ferrous sulfate, replacing the air with an inert gas, and then heating the base film for reaction, taking it out and washing it with water for 3-6 times, and then drying it to obtain a high-strength base film for a composite current collector; The preparation method of the modified PET resin comprises the following steps: adding 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin and catalyst into an organic solvent, stirring and reacting for 1-3 hours in an ice-water bath, then heating to 90-110° C., continuing stirring and reacting for 4-6 hours, cooling to room temperature, rotary evaporating to remove the solvent, and then washing and vacuum drying in sequence to obtain the modified PET resin; the mass ratio of the 5-methyl-3-phenyl-4-isoxazolecarbonyl chloride, pentafluorobenzoyl chloride, PET resin, catalyst and organic solvent is (6-8):(3-5):(70-90):(8-10):(250-350).

2. The high-strength base film for a composite current collector according to claim 1, characterized in that: The brand of the PET resin is PET CZ-333; the catalyst is anhydrous aluminum chloride; and the organic solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide, and N-methylpyrrolidone.

3. The high-strength base film for a composite current collector according to claim 1, characterized in that: The PP resin is PP F1002; the compatibilizer is compatibilizer CMG9801; the antioxidant is at least one of antioxidant 1010, antioxidant 168, and antioxidant 1076; the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570; and the lubricant is at least one of ethylene bis stearamide and butyl stearate.

4. The high-strength base film for a composite current collector according to claim 1, characterized in that: The fiber reinforcement material is glass fiber; the glass fiber is alkali-free glass fiber with an average diameter of 3-6 μm and a length of 1-3 mm; the filler is a mixture of aluminum hydroxide flame retardant VK-LA50, aluminum powder and copper powder in a mass ratio of 1:(2-4):3; the particle size of the filler is 1200-1600 mesh.

5. The high-strength base film for a composite current collector according to claim 1, characterized in that: The extrusion temperature of the twin-screw extruder in step S1 is 230-260°C, and the screw speed is 110-220 rpm; the biaxial stretching process in step S2 is specifically: the stretching temperature is 115-120°C, the stretching rate is 110-80mm / s, the heat setting temperature is 215-235°C, and the stretching ratio is 4:

1.

6. The high-strength base film for a composite current collector according to claim 1, characterized in that: The polar solvent in step S3 is at least one of N,N-dimethylformamide, dimethyl sulfoxide, and N,N-dimethylacetamide; the radiation is carried out in an air atmosphere at room temperature, and is continuous electron beam radiation with an absorbed dose of 50 to 350 kGy, a beam current of 10 to 90 mA, and a voltage of 180 to 430 kV.

7. The high-strength base film for a composite current collector according to claim 1, characterized in that: The mass ratio of the polar solvent, 1-allyl-3-vinylimidazolium chloride and ammonium ferrous sulfate in step S3 is (3-6):1:(0.03-0.05); the inert gas in step S3 is any one of nitrogen, helium, neon and argon; the reaction temperature of the heating reaction in step S3 is 60-75° C. and the time is 4-8 h.

Citation Information

Patent Citations

  • Polypropylene film and preparation method thereof, composite current collector, electrode sheet and application thereof

    CN117261303B

  • High-strength polyester film and preparation method thereof

    CN117624851A

  • MLCC release film base film and preparation method thereof

    CN117863696A