Recycling method of waste polyurethane material
Surface activation and molding of waste polyurethane materials through solid-phase shear grinding and high-temperature decross-linking technology, combined with waste rubber powder, solves the problems of difficulty in recycling polyurethane materials and environmental pollution in the existing technology, and achieves high efficiency and low cost. The excellent properties of polyurethane material recycling and composite materials.
Patent Information
- Application Number
- CN202411028365.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-15
AI Technical Summary
Existing technology makes it difficult to effectively recycle and reuse cross-linked waste polyurethane materials, resulting in their incineration or landfill, causing environmental pollution, and existing methods are inefficient, costly, or energy-intensive.
The polyurethane foam is pulverized using solid-phase shear grinding technology to activate its surface, and the polyurethane elastomer is processed through high-temperature decomposition and cross-linking. After uniform mixing, compression molding is performed to form a composite material. The surface-activated waste rubber powder is used As a modified filler, it improves the mechanical properties and hydrophobic properties of composite materials.
It achieves efficient recycling and reuse of polyurethane materials, with simple process, low cost and little environmental pollution, improves the recycling rate and economic benefits of materials, reduces the use of chemical solvents, and improves the mechanical properties and hydrophobic properties of composite materials.
Smart Images

Figure CN118772483A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical engineering, and in particular relates to a method for recycling waste polyurethane materials. Background Art
[0002] Polyurethane is a polymer material formed by the condensation reaction of polyols and polyisocyanates. By adjusting the types of raw materials, the ratio of hard and soft segments, and the synthesis process, the main chain structure of polyurethane molecules can be designed to meet the needs of different application scenarios, such as polyurethane foam, polyurethane adhesive, polyurethane coating, polyurethane elastomer, etc. Due to its diverse morphological structures and excellent material properties, polyurethane has been widely used in daily consumer goods, construction, medical, military, agriculture and other fields. For example, in the footwear industry, polyurethane elastomers are widely used to make soles and insoles due to their wear resistance, compression resistance and shock absorption; while polyurethane foam is widely used as a filling material for shoes due to its resilience, shock absorption and light weight and high strength to improve the comfort and stability of shoes. These wide applications have led to a continuous increase in the demand for polyurethane. However, with the expansion of polyurethane consumption and production scale, the accumulation of its waste is also increasing rapidly. Therefore, reducing the impact of polyurethane waste on the environment and improving resource utilization efficiency are crucial to promoting the sustainable development of my country's economy.
[0003] Most waste polyurethanes are typical cross-linked polymers, and their three-dimensional cross-linked network structure gives them excellent mechanical properties and stability. However, this structure also reduces their reprocessing and molding capabilities, which brings great difficulties to the recycling of waste polyurethane materials. Due to the difficulty and high cost of recycling, cross-linked waste polyurethanes are usually treated by incineration or landfill, which has caused serious damage to the ecological environment. Therefore, it is of great significance to study the recycling technology of thermosetting polyurethanes. At present, there are reports on the recycling methods of cross-linked waste polyurethanes, including physical recycling, chemical recycling, biodegradation recycling and pyrolysis recycling. However, these methods face many challenges due to imperfect technology or insufficient equipment. For example, the physical recycling method has the problems of low efficiency, high energy consumption and cost; the chemical recycling method faces the challenges of large-scale solvent use, harmful substance emissions and reduced quality and stability of recycled products; the problem of biodegradation recycling method is harsh conditions and incomplete degradation; pyrolysis recycling is usually accompanied by large energy consumption and toxic gas emissions. Summary of the invention
[0004] The purpose of the embodiment of the present invention is to provide a method for recycling waste polyurethane materials, which has simple process, convenient operation, high recovery rate, low recovery cost and little pollution to the environment.
[0005] The embodiment of the present invention is achieved as follows:
[0006] An embodiment of the present invention provides a method for recycling waste polyurethane materials, wherein the waste polyurethane materials include polyurethane foam and polyurethane elastomer. The method comprises the following steps:
[0007] S1: The polyurethane foam is crushed by solid phase shear grinding technology to activate its surface;
[0008] S2: The polyurethane elastomer is first crushed and then subjected to high temperature de-crosslinking treatment;
[0009] S3: uniformly mixing the surface activated polyurethane foam and the high temperature de-crosslinked polyurethane elastomer, wherein the mass distribution ratio of the polyurethane foam to the polyurethane elastomer is: 10%-90% of the polyurethane foam and 10%-90% of the polyurethane elastomer;
[0010] S4: The mixture uniformly mixed in step S3 is compression molded to obtain a composite material that can be reused.
[0011] Furthermore, in step S1, the grinding temperature is 20°C-40°C, the grinding disc speed of the grinding equipment is 200prm-600prm, and the number of cycle grinding is 1-25 times.
[0012] Furthermore, in step S2, a powerful pulverizer is used for pulverization, the pulverization temperature is 20°C-40°C, the high temperature cross-linking processing temperature is 140°C-190°C, and the processing time is 5-15 minutes.
[0013] Furthermore, in step S3, the mixing temperature is 140° C.-190° C., and the mixing time is 5-15 min.
[0014] Furthermore, in step S4, a flat plate vulcanizer is used for processing, and the material is preheated for 3-10 minutes at a temperature of 140°C-190°C. After the material is softened, a pressure of 10-15MPa is applied for 5-15min.
[0015] Furthermore, waste rubber powder can be added in step S3, and the mass distribution ratio of polyurethane foam, polyurethane elastomer and waste rubber powder is: polyurethane foam 10%-90%, polyurethane elastomer 10%-90%, waste rubber powder 1%-20%.
[0016] Furthermore, the polyurethane foam and the waste rubber powder are firstly mixed uniformly with a high-speed stirrer, and then the mixture is mixed uniformly with the polyurethane elastomer with a rotational rheometer, an internal mixer or a screw extruder to obtain the corresponding compound.
[0017] Furthermore, the stirring speed of the high-speed stirrer is 28000 prm, and the stirring time is 1-5 min.
[0018] The beneficial effects of the present invention are:
[0019] The method for recycling and reusing waste polyurethane materials provided by the embodiment of the present invention has a simple process, convenient operation, high recovery rate, low recovery cost, and little pollution to the environment. The entire recycling process does not require the addition of any organic solvent, which reduces the pollution of chemical substances to the environment and meets the development needs of low-carbon and environmental protection. The selected waste polyurethane materials and raw materials such as waste rubber powder are all from waste, which can bring significant economic benefits and market competitive advantages.
[0020] The solid-phase force chemical grinding method was used to reduce the particle size of waste polyurethane foam particles and improve their surface activity, thereby enhancing their compatibility and dispersibility in other polymer matrices; the processing fluidity of waste polyurethane elastomer particles was improved through high-temperature decrosslinking; and the comprehensive utilization of two waste polyurethane materials with different structures was achieved through thermal processing.
[0021] Selecting waste rubber powder after surface activation treatment as modified filler can improve the mechanical properties and hydrophobic properties of the composite material and enhance the utilization value of the waste rubber powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 This is the microscopic morphology of polyurethane foam particles under a scanning electron microscope;
[0024] Figure 2 The Fourier transform infrared spectra of the unground polyurethane foam particles and the polyurethane foam particles ground 5 times;
[0025] Figure 3 This is the cross-sectional microscopic morphology of the PUS / PUF composite material under an electron microscope;
[0026] Figure 4 This is the test result diagram of PUS / PUF / mRP composite material under SEM-EDS;
[0027] Figure 5 The curve diagram of the torque of polyurethane elastomer de-crosslinking at different temperatures versus time;
[0028] Figure 6 is the tensile performance diagram of PUS / PUF composite material;
[0029] Figure 7 is the tensile performance diagram of PUS / PUF / mRP composites;
[0030] Figure 8 The hydrophobic performance diagram of the composite material. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0032] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.
[0034] In this application, waste polyurethane materials mainly refer to polyurethane foam (PUF) and polyurethane elastomer (PUS). Polyurethane foam refers to polyurethane waste produced due to backward production technology or improper storage conditions, resulting in product performance that does not meet the use requirements. According to the composition of raw materials, it can be divided into polyether polyurethane foam, polyester polyurethane foam, polyurea polyurethane foam and thermoplastic polyurethane foam, etc. Polyurethane elastomer refers to polyurethane waste produced due to backward production technology or improper storage conditions, resulting in product performance that does not meet the use requirements. According to the composition of raw materials, it can be divided into polyether polyurethane elastomer, polyester polyurethane elastomer, polyurea polyurethane elastomer and thermoplastic polyurethane elastomer, etc.
[0035] Example 1
[0036] Embodiment 1 of the present invention provides a method for recycling waste polyurethane materials, comprising the following steps:
[0037] S1: The polyurethane foam is crushed by solid phase shear grinding technology to activate its surface.
[0038] In this step, 1 kg of waste polyurethane foam is placed in a solid phase force chemical reactor and cyclically ground for 5 times at room temperature. During grinding, the grinding disc speed is set to 400 rpm and the pressure is set to 1.0 MPa, thereby obtaining surface-activated polyurethane foam particles.
[0039] S2: The polyurethane elastomer is first crushed and then subjected to high temperature de-crosslinking treatment.
[0040] In this step, the polyurethane elastomer is crushed with a powerful crusher, and then 40g of the crushed and dried waste polyurethane elastomer particles are added to an internal mixer for decrosslinking. During processing, the rotor speed is set to 60prm, the processing temperature is 170°C, and the processing time is 10min to obtain decrosslinked polyurethane elastomer particles.
[0041] It should be noted that, in this step, a rotational rheometer or a screw extruder may also be used to perform high temperature cross-linking.
[0042] S3: uniformly mixing the surface activated polyurethane foam and the high temperature de-crosslinked polyurethane elastomer, wherein the mass distribution ratio of the polyurethane foam to the polyurethane elastomer is: 10%-90% of the polyurethane foam and 10%-90% of the polyurethane elastomer.
[0043] In this embodiment, 4 g of surface-activated polyurethane foam particles and 36 g of de-crosslinked polyurethane elastomer particles are added to an internal mixer for mixing. During processing, the rotor speed is set to 60prm, the processing temperature is set to 170°C, and the processing time is set to 10 min to obtain a mixture of polyurethane foam and polyurethane elastomer.
[0044] S4: The mixture uniformly mixed in step S3 is compression molded to obtain a composite material that can be reused.
[0045] In this step, the mixed material obtained in the previous step is added to a flat vulcanizer and preheated for 5 minutes. The preheating temperature is set to 140°C to fully soften the mixed material. Then, the hot pressing temperature is set to 170°C, the compression pressure is 10 MPa, and the hot pressing time is 15 minutes, thereby compression molding to obtain a PUS / PUF composite material.
[0046] Example 2
[0047] Embodiment 2 of the present invention provides a method for recycling waste polyurethane materials, comprising the following steps:
[0048] S1: The polyurethane foam is crushed by solid phase shear grinding technology to activate its surface.
[0049] In this step, 1 kg of waste polyurethane foam is placed in a solid phase force chemical reactor and cyclically ground for 5 times at room temperature. During grinding, the grinding disc speed is set to 400 rpm and the pressure is set to 1.0 MPa, thereby obtaining surface-activated polyurethane foam particles.
[0050] S2: The polyurethane elastomer is first crushed and then subjected to high temperature de-crosslinking treatment.
[0051] In this step, the polyurethane elastomer is crushed with a powerful crusher, and then 40g of the crushed and dried waste polyurethane elastomer particles are added to an internal mixer for decrosslinking. During processing, the rotor speed is set to 60prm, the processing temperature is 180°C, and the processing time is 10min to obtain decrosslinked polyurethane elastomer particles.
[0052] S3: uniformly mixing the surface activated polyurethane foam and the high temperature de-crosslinked polyurethane elastomer, wherein the mass distribution ratio of the polyurethane foam to the polyurethane elastomer is: 10%-90% of the polyurethane foam and 10%-90% of the polyurethane elastomer.
[0053] In this embodiment, 4 g of surface-activated polyurethane foam particles and 36 g of de-crosslinked polyurethane elastomer particles are added to an internal mixer for mixing. During processing, the rotor speed is set to 60prm, the processing temperature is set to 170°C, and the processing time is set to 10 min to obtain a mixture of polyurethane foam and polyurethane elastomer.
[0054] S4: The mixture uniformly mixed in step S3 is compression molded to obtain a composite material that can be reused.
[0055] In this step, the mixed material obtained in the previous step is added to a flat vulcanizer and preheated for 5 minutes. The preheating temperature is set to 140°C to fully soften the mixed material. Then, the hot pressing temperature is set to 170°C, the compression pressure is 10 MPa, and the hot pressing time is 15 minutes, thereby compression molding to obtain a PUS / PUF composite material.
[0056] Example 3
[0057] Embodiment 3 of the present invention provides a method for recycling waste polyurethane materials, comprising the following steps:
[0058] S1: The polyurethane foam is crushed by solid phase shear grinding technology to activate its surface.
[0059] In this step, 1 kg of waste polyurethane foam is placed in a solid phase force chemical reactor and cyclically ground for 5 times at room temperature. During grinding, the grinding disc speed is set to 400 rpm and the pressure is set to 1.0 MPa, thereby obtaining surface-activated polyurethane foam particles.
[0060] S2: The polyurethane elastomer is first crushed and then subjected to high temperature de-crosslinking treatment.
[0061] In this step, the polyurethane elastomer is crushed with a powerful crusher, and then 40g of the crushed and dried waste polyurethane elastomer particles are added to an internal mixer for decrosslinking. During processing, the rotor speed is set to 60prm, the processing temperature is 190°C, and the processing time is 10min to obtain decrosslinked polyurethane elastomer particles.
[0062] S3: uniformly mixing the surface activated polyurethane foam and the high temperature de-crosslinked polyurethane elastomer, wherein the mass distribution ratio of the polyurethane foam to the polyurethane elastomer is: 10%-90% of the polyurethane foam and 10%-90% of the polyurethane elastomer.
[0063] In this embodiment, 4 g of surface-activated polyurethane foam particles and 36 g of de-crosslinked polyurethane elastomer particles are added to an internal mixer for mixing. During processing, the rotor speed is set to 60prm, the processing temperature is set to 170°C, and the processing time is set to 10 min to obtain a mixture of polyurethane foam and polyurethane elastomer.
[0064] S4: The mixture uniformly mixed in step S3 is compression molded to obtain a composite material that can be reused.
[0065] In this step, the mixed material obtained in the previous step is added to a flat vulcanizer and preheated for 5 minutes. The preheating temperature is set to 140°C to fully soften the mixed material. Then, the hot pressing temperature is set to 170°C, the compression pressure is 10 MPa, and the hot pressing time is 15 minutes, thereby compression molding to obtain a PUS / PUF composite material.
[0066] Example 4
[0067] Embodiment 4 of the present invention provides a method for recycling waste polyurethane materials, comprising the following steps:
[0068] S1: The polyurethane foam is crushed by solid phase shear grinding technology to activate its surface.
[0069] In this step, 1 kg of waste polyurethane foam is placed in a solid phase force chemical reactor and cyclically ground for 25 times at 40° C. The grinding disc speed is set to 200 rpm and the pressure is set to 1.0 MPa during grinding, thereby obtaining surface-activated polyurethane foam particles.
[0070] S2: The polyurethane elastomer is first crushed and then subjected to high temperature de-crosslinking treatment.
[0071] In this step, the polyurethane elastomer is crushed with a powerful crusher, and then 40g of the crushed and dried waste polyurethane elastomer particles are added to an internal mixer for decrosslinking. During processing, the rotor speed is set to 60prm, the processing temperature is 140°C, and the processing time is 15min to obtain decrosslinked polyurethane elastomer particles.
[0072] S3: uniformly mixing the surface activated polyurethane foam and the high temperature de-crosslinked polyurethane elastomer, wherein the mass distribution ratio of the polyurethane foam to the polyurethane elastomer is: 10%-90% of the polyurethane foam and 10%-90% of the polyurethane elastomer.
[0073] In this embodiment, 36 g of surface-activated polyurethane foam particles and 4 g of de-crosslinked polyurethane elastomer particles are added to an internal mixer for mixing. During processing, the rotor speed is set to 60prm, the processing temperature is set to 190°C, and the processing time is set to 5 minutes to obtain a mixture of polyurethane foam and polyurethane elastomer.
[0074] S4: The mixture uniformly mixed in step S3 is compression molded to obtain a composite material that can be reused.
[0075] In this step, the mixed material obtained in the previous step is added to a flat vulcanizer and preheated for 3 minutes. The preheating temperature is set to 140°C to fully soften the mixed material. Then, the hot pressing temperature is set to 190°C, the compression pressure is 15 MPa, and the hot pressing time is 5 minutes, thereby compression molding to obtain a PUS / PUF composite material.
[0076] Example 5
[0077] Embodiment 5 of the present invention provides a method for recycling waste polyurethane materials, comprising the following steps:
[0078] S1: The polyurethane foam is crushed by solid phase shear grinding technology to activate its surface.
[0079] In this step, 1 kg of waste polyurethane foam is placed in a solid phase force chemical reactor and cyclically ground for 15 times at 30° C. The grinding disc speed is set to 600 rpm and the pressure is set to 1.0 MPa during grinding, thereby obtaining surface-activated polyurethane foam particles.
[0080] S2: The polyurethane elastomer is first crushed and then subjected to high temperature de-crosslinking treatment.
[0081] In this step, the polyurethane elastomer is crushed with a powerful crusher, and then 40g of the crushed and dried waste polyurethane elastomer particles are added to an internal mixer for decrosslinking. During processing, the rotor speed is set to 60prm, the processing temperature is 190°C, and the processing time is 5min to obtain decrosslinked polyurethane elastomer particles.
[0082] S3: uniformly mixing the surface activated polyurethane foam and the high temperature de-crosslinked polyurethane elastomer, wherein the mass distribution ratio of the polyurethane foam to the polyurethane elastomer is: 10%-90% of the polyurethane foam and 10%-90% of the polyurethane elastomer.
[0083] In this embodiment, 20 g of surface-activated polyurethane foam particles and 20 g of de-crosslinked polyurethane elastomer particles are added to an internal mixer for mixing. During processing, the rotor speed is set to 60prm, the processing temperature is set to 140°C, and the processing time is set to 15min to obtain a mixture of polyurethane foam and polyurethane elastomer.
[0084] S4: The mixture uniformly mixed in step S3 is compression molded to obtain a composite material that can be reused.
[0085] In this step, the mixed material obtained in the previous step is added to a flat vulcanizer and preheated for 3 minutes. The preheating temperature is set to 140°C to fully soften the mixed material. Then, the hot pressing temperature is set to 150°C, the compression pressure is 12 MPa, and the hot pressing time is 10 minutes, thereby compression molding to obtain a PUS / PUF composite material.
[0086] Example 6
[0087] Embodiment 6 of the present invention provides a method for recycling waste polyurethane materials, comprising the following steps:
[0088] S1: The polyurethane foam is crushed by solid phase shear grinding technology to activate its surface.
[0089] In this step, 1 kg of waste polyurethane foam is placed in a solid phase force chemical reactor and cyclically ground for 10 times at room temperature. During the grinding, the grinding disc speed is set to 400 rpm and the pressure is set to 1.0 MPa, thereby obtaining surface-activated polyurethane foam particles.
[0090] S2: The polyurethane elastomer is first crushed and then subjected to high temperature de-crosslinking treatment.
[0091] In this step, the polyurethane elastomer is crushed with a powerful crusher, and then 40g of the crushed and dried waste polyurethane elastomer particles are added to an internal mixer for decrosslinking. During processing, the rotor speed is set to 60prm, the processing temperature is 170°C, and the processing time is 15min to obtain decrosslinked polyurethane elastomer particles.
[0092] S3: The surface activated polyurethane foam, the high temperature de-crosslinked polyurethane elastomer and the waste rubber powder (mRP) are uniformly mixed, and the mass distribution ratio of the polyurethane foam, the polyurethane elastomer and the waste rubber powder is: polyurethane foam 10%-90%, polyurethane elastomer 10%-90%, and waste rubber powder 1%-20%.
[0093] In this embodiment, 100g of surface activated polyurethane foam particles and 100g of surface activated waste rubber powder are stirred in a high-speed stirrer for 5min at a stirring speed of 28000prm to ensure that the two are evenly mixed. Then 20g of the mixed material is taken, and 20g of de-crosslinked polyurethane elastomer particles are added to an internal mixer for mixing. During processing, the rotor speed is set to 60prm, the processing temperature is 170°C, and the processing time is 10min to obtain the corresponding mixed material.
[0094] S4: The mixed material uniformly mixed in step S3 is compression molded to obtain a composite material that can be reused.
[0095] In this step, the mixed material obtained in the previous step is added to a flat vulcanizer and preheated for 5 minutes. The preheating temperature is set to 140°C to fully soften the mixed material. Then, the hot pressing temperature is set to 170°C, the compression pressure is 10 MPa, and the hot pressing time is 15 minutes, thereby compression molding to obtain a PUS / PUF / mRP composite material.
[0096] Example 7
[0097] Embodiment 7 of the present invention provides a method for recycling waste polyurethane materials, comprising the following steps:
[0098] S1: The polyurethane foam is crushed by solid phase shear grinding technology to activate its surface.
[0099] In this step, 1 kg of waste polyurethane foam is placed in a solid phase force chemical reactor and cyclically ground for 5 times at room temperature. During grinding, the grinding disc speed is set to 400 rpm and the pressure is set to 1.0 MPa, thereby obtaining surface-activated polyurethane foam particles.
[0100] S2: The polyurethane elastomer is first crushed and then subjected to high temperature de-crosslinking treatment.
[0101] In this step, the polyurethane elastomer is crushed with a powerful crusher, and then 40g of the crushed and dried waste polyurethane elastomer particles are added to an internal mixer for decrosslinking. During processing, the rotor speed is set to 60prm, the processing temperature is 170°C, and the processing time is 15min to obtain decrosslinked polyurethane elastomer particles.
[0102] S3: The surface activated polyurethane foam, the high temperature de-crosslinked polyurethane elastomer and the waste rubber powder (mRP) are uniformly mixed, and the mass distribution ratio of the polyurethane foam, the polyurethane elastomer and the waste rubber powder is: polyurethane foam 10%-90%, polyurethane elastomer 10%-90%, and waste rubber powder 1%-20%.
[0103] In this embodiment, 160g of surface activated polyurethane foam particles and 40g of surface activated waste rubber powder were stirred in a high-speed stirrer for 5min at a stirring speed of 28000prm to ensure that the two were evenly mixed. Then 10g of the mixed material was taken, and 30g of de-crosslinked polyurethane elastomer particles were added to an internal mixer for mixing. During processing, the rotor speed was set to 60prm, the processing temperature was 170°C, and the processing time was 10min to obtain the corresponding mixed material.
[0104] S4: The mixed material uniformly mixed in step S3 is compression molded to obtain a composite material that can be reused.
[0105] In this step, the mixed material obtained in the previous step is added to a flat vulcanizer and preheated for 5 minutes. The preheating temperature is set to 140°C to fully soften the mixed material. Then, the hot pressing temperature is set to 170°C, the compression pressure is 10 MPa, and the hot pressing time is 15 minutes, thereby compression molding to obtain a PUS / PUF / mRP composite material.
[0106] Comparative Example 1
[0107] Comparative Example 1 provides a method for recycling and reusing waste polyurethane materials. The difference between this comparative example and Example 1 is that the polyurethane foam is not subjected to surface activation treatment.
[0108] The recycling method of this comparative example comprises the following steps:
[0109] S1: The polyurethane elastomer is crushed with a powerful crusher, and then 40 g of the crushed and dried waste polyurethane elastomer particles are added to an internal mixer for de-crosslinking. During processing, the rotor speed is set to 60 rpm, the processing temperature is 170°C, and the processing time is 15 min to obtain de-crosslinked polyurethane elastomer particles.
[0110] S2: 4 g of polyurethane foam particles that have not been surface activated and 36 g of de-crosslinked polyurethane elastomer particles are added to an internal mixer for mixing. During processing, the rotor speed is set to 60 rpm, the processing temperature is set to 170°C, and the processing time is set to 10 min to obtain a mixture of polyurethane foam and polyurethane elastomer.
[0111] S3: The mixed material obtained in the previous step is added to a flat vulcanizer and preheated for 5 minutes. The preheating temperature is set to 140°C to fully soften the mixed material. Then, the hot pressing temperature is set to 170°C, the compression pressure is 10 MPa, and the hot pressing time is 15 minutes, thereby compression molding to obtain a PUS / PUF composite material.
[0112] Experimental analysis
[0113] 1. Characterization and Analysis
[0114] The chemical structure and microscopic morphology of the material were characterized and analyzed accordingly, and the results are as follows:
[0115] 1. Reference Figure 1As shown, Figure a is the microscopic morphology of the unground polyurethane foam particles under a scanning electron microscope, Figure b is the microscopic morphology of the polyurethane foam particles ground 5 times under a scanning electron microscope, Figure c is the microscopic morphology of the polyurethane foam particles ground 10 times under a scanning electron microscope, and Figure d is the microscopic morphology of the polyurethane foam particles ground 15 times under a scanning electron microscope. It can be seen from the figures that with the increase in the number of grinding times, the particle size of the polyurethane foam particles gradually decreases and the size distribution becomes more uniform.
[0116] 2. Reference Figure 2 As shown in the figure, it is the Fourier infrared spectra of the unground polyurethane foam particles (PUF-0) and the polyurethane foam particles ground 5 times (PUF-5). From the analysis of the figure, it can be seen that grinding destroys the original cross-linked structure of the polyurethane foam particles, and more active groups are exposed on the surface of the particles, thereby enhancing the surface activity of the particles.
[0117] 3. Reference Figure 3 As shown, it is Comparative Example 1 ( Figure 3 a) and Example 1 ( Figure 3 b) Cross-sectional microscopic morphology of the prepared PUS / PUF composite material under an electron microscope. It can be seen from the figure that the dispersion and compatibility of the ground PUF particles in the PUS matrix are significantly improved compared with the untreated PUF particles.
[0118] 4. Reference Figure 4 As shown in the figure, it is the test result of PUS / PUF / mRP composite material under SEM-EDS, which is used to analyze the interface compatibility of the composite material and the dispersion of mRP in PUS. Figure a and Figure b are the brittle fracture morphology of the composite material with mRP filling amount of 10wt% and 20wt%, respectively. In order to further analyze the dispersion of mRP in PUS, EDS is used to characterize the element distribution of sulfur element in the fracture section, and the results are shown in Figure c and Figure d. It can be seen that no agglomeration or pores appear in the composite materials with different mRP filling amounts, and the sulfur element is evenly distributed in the PUS matrix, indicating that mRP and PUF have good compatibility and dispersibility in the composite material.
[0119] 2. Performance Test
[0120] 1. Test methods
[0121] (1) Processability: The torque of the crushed PUS particles at different temperatures was analyzed over time using a torque rheometer to evaluate the effect of processing temperature on the processing performance of PUS.
[0122] (2) Mechanical properties: The tensile properties of the composite materials were tested using a universal material testing machine in accordance with GB / T528-2009.
[0123] (3) Hydrophobicity: The water contact angle of the composite material was tested using an optical contact angle analyzer to evaluate the effect of mRP on the hydrophobicity of the material surface.
[0124] 2. Test results
[0125] refer to Figure 5 As shown in the figure, it is the change curve of the torque of the polyurethane elastomer at different temperatures over time. It can be seen from the figure that at different temperatures, the torque of the material after stabilization is basically the same; but as the temperature increases, the material torque can stabilize faster, which shows that increasing the temperature helps to improve the processability of the material.
[0126] refer to Figure 6 As shown in the figure, it is a tensile performance diagram of PUS / PUF composite materials under different conditions, which is used to analyze the influence of the filling amount of PUF-5 and the number of grinding times during the PUF surface activation treatment on the tensile properties of the composite materials. Figures a and b are stress-strain curves and tensile strength diagrams when the polyurethane foam content in the PUS / PUF composite material is 5%, 10%, 15%, and 20% respectively when the polyurethane foam is ground 5 times, and Figures c and d are stress-strain curves and tensile strength diagrams when the polyurethane foam content is 10% and the grinding times are 0, 1, 3, and 5 times respectively. It can be seen from Figures a and b that with the increase of PUF-5 filling amount, the tensile strength and elongation at break of the composite material show a trend of increasing first and then decreasing. This is because the PUF after surface activation treatment has good dispersibility and compatibility in the matrix, and a good interface interaction will be formed between the two. At the same time, compared with PUS, PUF has a lower molecular weight, which can play a certain degree of plasticizing effect, improve the molding ability of PUS during melt processing, reduce the density of defects such as uneven microstructure or stress concentration formed during material molding, and improve the performance of the material. However, there are still certain differences between PUF and PUS uncrosslinked parts, so as to increase the PUF-5 filling amount, the component uniformity of the composite material decreases, which leads to a decrease in the tensile strength of the composite material. Combining the results of Figure c and Figure d, it can be seen that when the PUF filling amount is constant, the tensile strength of the composite material increases with the increase in the number of PUF grinding times. This is because the grinding treatment not only helps to further refine the PUF particle size, thereby improving its dispersibility in the matrix; at the same time, grinding promotes the de-crosslinking of PUF, thereby increasing its surface activity and thereby enhancing its interaction with the matrix; in addition, the grinding treatment helps to enhance the segmental motion activity of the PUF molecular chain, which is beneficial to its mutual entanglement and embedding with the PUS molecular chain during the melt processing, thereby enhancing the interface interaction.
[0127] refer to Figure 7As shown in the figure, it is a tensile performance diagram of PUS / PUF / mRP composite materials under different conditions. Figure a is a stress-strain curve diagram of waste rubber powder (mRP) content of 5%, 10%, 15%, and 20%, respectively, and Figure b is the corresponding tensile strength diagram. From the analysis of the figure, it can be seen that the mechanical properties of the composite material are significantly improved after the introduction of mRP. This is mainly attributed to the small and uniformly distributed particle size of mRP, which makes it have good dispersion in the matrix. In addition, the oxygen-containing polar functional groups on the surface of mRP form a strong interaction with the polyurethane matrix, thereby further enhancing the performance of the composite material.
[0128] refer to Figure 8 As shown, it is a graph of the hydrophobic performance of the composite material. Figure a is a PUS / PUF composite material that has been ground 5 times in polyurethane foam (PUF-5), with a filling amount of 10wt% and no mRP added. Figures b-e are PUS / PUF / mRP composite materials with mRP contents of 5%, 10%, 15%, and 20% added, respectively. As can be seen from the figure, the water contact angle of the PUS / PUF composite material without the introduction of mRP is 75.2°, showing hydrophilicity. This is because the polyurethane itself contains polar groups and has a high surface energy. As the mRP filling amount increases, the hydrophobicity of the composite material gradually increases. When the mRP addition amount increases to 20wt%, the water contact angle of the PUS / PUF / mRP composite material reaches 105.4°, showing hydrophobicity. This is because the rubber powder itself has few polar groups, strong hydrophobicity, and stable chemical properties. Excellent hydrophobicity will help improve the stability of polyurethane materials in humid environments or rainwater and extend the service life of the materials. At the same time, the improvement of hydrophobicity can prevent the penetration of water and other substances, reduce the adhesion of some pollutants, and make the material easier to clean and maintain. Therefore, the introduction of mRP to improve the hydrophobicity of composite materials will give the material a wider application space in the footwear industry and other fields.
[0129] The present invention is not limited to the above optional implementation modes. Anyone can derive other implementation modes under the enlightenment of the present invention. All technical solutions falling within the scope defined by the claims of the present invention fall within the protection scope of the present invention.
Claims
1. A method for recycling and reusing waste polyurethane materials, wherein the waste polyurethane materials include polyurethane foam and polyurethane elastomer, characterized in that: The method comprises the following steps, S1: The polyurethane foam is crushed by solid phase shear grinding technology to activate its surface; S2: The polyurethane elastomer is first crushed and then subjected to high-temperature de-crosslinking treatment; S3: uniformly mixing the surface-activated polyurethane foam and the high-temperature cross-linked polyurethane elastomer, wherein the mass distribution ratio of the polyurethane foam to the polyurethane elastomer is: 10%-90% polyurethane foam, 10%-90% polyurethane elastomer; S4: The mixture uniformly mixed in step S3 is compression molded to obtain a composite material that can be reused.
2. The method for recycling and reusing waste polyurethane materials according to claim 1, characterized in that: In step S1, the grinding temperature is 20° C.-40° C., the grinding disc speed of the grinding equipment is 200 rpm-600 rpm, and the number of cycle grinding is 1-25 times.
3. The method for recycling and reusing waste polyurethane materials according to claim 1, wherein: In step S2, a powerful pulverizer is used for pulverization, the pulverization temperature is 20° C.-40° C., the high-temperature de-crosslinking processing temperature is 140° C.-190° C., and the processing time is 5-15 minutes.
4. The method for recycling and reusing waste polyurethane materials according to claim 1, wherein: In step S3, the mixing temperature is 140° C.-190° C., and the mixing time is 5-15 minutes.
5. The method for recycling and reusing waste polyurethane materials according to claim 1, characterized in that: In step S4, a flat plate vulcanizer is used for processing, and the material is preheated for 3-10 minutes at a temperature of 140°C-190°C. After the material is softened, a pressure of 10-15 MPa is applied for 5-15 minutes.
6. The method for recycling and reusing waste polyurethane materials according to claim 1, characterized in that: In step S3, waste rubber powder can also be added. The mass distribution ratio of polyurethane foam, polyurethane elastomer and waste rubber powder is: polyurethane foam 10%-90%, polyurethane elastomer 10%-90%, waste rubber powder 1%-20%.
7. The method for recycling and reusing waste polyurethane materials according to claim 6, characterized in that: First, the polyurethane foam and the waste rubber powder are mixed evenly with a high-speed stirrer, and then the mixture is mixed evenly with the polyurethane elastomer with a rotational rheometer, an internal mixer or a screw extruder to obtain the corresponding compound.
8. The method for recycling and reusing waste polyurethane materials according to claim 7, characterized in that: The stirring speed of the high-speed stirrer is 28000rpm, and the stirring time is 1-5min.