Composite aluminum oxide as well as preparation method and application thereof

CN118772485APending Publication Date: 2024-10-15YAAN BESTRY PERFORMANCE MATERIALS CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410785173.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Among existing thermally conductive materials, spherical alumina requires a high filling rate to obtain high thermal conductivity, but this will affect the viscosity and processability of the organic matrix, and the thermal conductivity and mechanical properties of flaky alumina decrease when they are piled up disorderly. Difficulty meeting demand.

Method used

Composite alumina is prepared by depositing Fe3O4 on the surface of flaky alumina, and orienting it under the induction of an external magnetic field to increase the contact heat transfer area, reduce the filling rate to increase thermal conductivity, and reduce the impact on the organic matrix.

Benefits of technology

Achieve high thermal conductivity at low filling rates, reduce the impact on the viscosity and processability of the organic matrix, and improve the performance of thermally conductive materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772485A_ABST
    Figure CN118772485A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of inorganic heat-conducting materials, and discloses composite aluminum oxide as well as a preparation method and application thereof. The preparation method of the composite aluminum oxide comprises the following steps: S1, mixing flaky aluminum oxide powder with deionized water, heating, stirring and dispersing to obtain a mixed solution A; s2, adding a mixed solution of ferric salt and ferrous salt into the mixed solution A, uniformly mixing, and slowly adding ammonia water to adjust the pH to be alkaline, so as to obtain a mixed solution B; and S3, filtering, washing and drying the precipitate in the mixed solution B to obtain the composite alumina powder. The composite aluminum oxide is formed by coating the surface of flaky aluminum oxide with a thin layer of Fe3O4, when the composite aluminum oxide is applied to a heat-conducting material of electronic equipment and the filling rate is 20-60%, relatively high heat conductivity can be obtained, and the influence on physical properties such as viscosity and machinability of an organic matrix in the heat-conducting material can be effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of inorganic thermal conductive materials, and in particular to composite aluminum oxide and a preparation method and application thereof. Background Art

[0002] With the development of Internet technology, electronic devices are everywhere in our lives, and the heating problem of electronic devices during use has led to an increasing demand for thermal conductive materials in the industry. Among the current mainstream thermal conductive materials, spherical alumina is the main thermal conductive medium, and spherical alumina often needs to be compounded and use a high filling rate to obtain high thermal conductivity. High filling materials will affect the physical properties of the organic matrix, such as viscosity and processability.

[0003] It is known that flaky aluminum oxide has a larger and wider contact surface. However, when it is added to an organic matrix for compounding thermal conductive materials, the flaky aluminum oxide tends to be disorderly stacked, which reduces the thermal conductivity and mechanical properties and makes it difficult to meet the current demand for thermal conductive materials. Summary of the invention

[0004] The purpose of the present invention is to provide a composite alumina and a preparation method and application thereof in view of the defects of the prior art. The composite alumina prepared by the method is characterized by depositing Fe3O4 on the surface of flaky alumina, so that the composite alumina has magnetism. Under the induction of an external magnetic field, the flaky composite alumina can be oriented to increase the contact heat transfer area. When used as a thermal conductive material, the filling rate of the composite alumina can be reduced and the thermal conductivity can be improved. In particular, a higher thermal conductivity can be obtained at a lower filling rate, while reducing the impact on the physical properties of the organic matrix in the thermal conductive material, such as viscosity and machinability.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] In one aspect, the present invention provides a method for preparing composite alumina, comprising the following steps:

[0007] S1, mixing flaky aluminum oxide powder with deionized water, heating, stirring and dispersing, to obtain a mixed solution A;

[0008] S2, adding a mixed solution of ferric salt and ferrous salt to the mixed solution A, mixing evenly, and then slowly adding ammonia water to adjust the pH to alkaline, to obtain a mixed solution B;

[0009] S3, filtering, washing and drying the precipitate in the mixed solution B to obtain composite alumina powder.

[0010] Preferably, the particle size D50 of the flaky aluminum oxide is 5-35 μm.

[0011] Preferably, the method for preparing the flaky aluminum oxide comprises the following steps:

[0012] P1, add boehmite powder into a composite molten salt aqueous solution of Na2SO4 and K2SO4, disperse evenly, and obtain a mixed solution C;

[0013] P2, adding trisodium phosphate and titanyl sulfate to the mixed solution C, stirring until completely dissolved, to obtain a mixed solution D;

[0014] P3, drying the mixed solution D, sintering, washing and drying the powder to obtain the flaky aluminum oxide.

[0015] Preferably, the mass ratio of the boehmite to the composite molten salt is 1:4;

[0016] And / or, the mass ratio of Na2SO4 to K2SO4 is 1:1;

[0017] And / or, the molten salt mass concentration of the composite molten salt aqueous solution is 300 g / L;

[0018] And / or, the amount of trisodium phosphate added is 2.5% of the mass of the boehmite powder, and the amount of titanyl sulfate added is 4% of the mass of the boehmite powder.

[0019] Preferably, the iron salt includes one or more of ferric sulfate, ferric nitrate, and ferric chloride;

[0020] And / or, the ferrous salt includes one or more of ferrous sulfate, ferrous nitrate, and ferrous chloride;

[0021] And / or, in the mixed solution of the ferric salt and the ferrous salt, the concentration of the iron ion is 0.5 mol / L, and the molar ratio of the ferric salt to the ferrous salt is 2:1;

[0022] And / or, the ratio of the total mass of the ferric salt and the ferrous salt to the mass of the flaky aluminum oxide is 0.5-3:1.

[0023] Preferably, in step S2, aqueous ammonia is added to adjust the pH to 12 to obtain a mixed solution B.

[0024] On the other hand, the present invention provides a composite alumina, which is prepared by any of the composite alumina preparation methods described above.

[0025] On the other hand, the present invention also provides a composite alumina, wherein the composite alumina is a flaky alumina surface coated with a thin layer of Fe3O4, wherein the mass content of Fe3O4 in the composite alumina is 0.5-5%; and the specific surface area of ​​the composite alumina is 4-30 m 2 / g.

[0026] In another aspect, the present invention provides an application of the composite alumina as described in any one of the above items, including an application of the composite alumina in thermal conductive materials for electronic devices.

[0027] Preferably, the filling rate of the composite alumina in the thermal conductive material is 20-60%;

[0028] And / or, during the preparation of the thermal conductive material, an external vertical magnetic field is applied to induce orientation treatment, the magnetic field strength is 400 mT, and the induction time is 0 to 120 min.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The composite alumina preparation method of the present application is to heat and disperse the flaky alumina in deionized water and then mix it with a mixed solution of iron salt and ferrous salt, and then adjust the pH with ammonia water to deposit Fe3O4 on the surface of the flaky alumina, and finally obtain flaky composite alumina (Fe3O4-Al2O3); the preparation method has mild process conditions and simple operation. The surface of the prepared composite alumina is coated with a thin layer of Fe3O4, which is magnetic and can be induced to orient under the action of an external magnetic field, so that when used as a thermal conductive filler, it can achieve directional arrangement, so that the prepared thermal conductive filler can have good thermal conductivity at a low filling rate of the composite alumina. That is, when the composite alumina of the present application is used to prepare a thermal conductive material, it can achieve the effect of high thermal conductivity at a low filling rate, and reduce the impact on the physical properties of the organic matrix in the thermal conductive material, such as viscosity and machinability.

[0031] 2. When conventional spherical alumina is used to make thermal conductive materials, its filling rate is usually 80% or more to effectively improve the thermal conductivity of epoxy resins and other materials and achieve thermal conductivity. When the filling rate is 20-60%, the thermal conductivity of epoxy resins and other materials is not greatly improved. When the filling rate is 60%, the thermal conductivity is less than 0.4 W / mK. Therefore, when the filling rate of spherical alumina is too low, a thermal conductive path cannot be formed, and filling is meaningless. When the composite alumina of the present application is used to make thermal conductive fillers, the thermal conductivity of the conductive material can be greatly improved at a low filling rate of 20%-60%, which has a good thermal conductive effect, and the low filling rate has less effect on the viscosity and processability of the organic matrix in the thermal conductive material.

[0032] 3. The composite alumina product of the present application has a Fe3O4 mass content controlled within the range of 0.5-5%, which can effectively ensure that the composite alumina product has responsiveness under a magnetic field and has good thermal conductivity, that is, the interface thermal resistance effect brought by the Fe3O4 coating is small, and the thermal conductivity is less affected; the specific surface area of ​​the composite alumina is controlled within the range of 4-30m 2 / g range, which can ensure that it has a high heat transfer efficiency and is suitable for use as a thermal conductive material for electronic equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 The process flow chart of the composite alumina preparation method of the present invention is shown in FIG.

[0035] Figure 2 This is a SEM image of the flaky aluminum oxide prepared in the present invention.

[0036] Figure 3 This is a SEM image of the composite alumina (Fe3O4-Al2O3) prepared in the present invention. DETAILED DESCRIPTION

[0037] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present invention. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.

[0038] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0039] The embodiment of the present invention provides a composite aluminum oxide and a preparation method and application thereof.

[0040] like Figure 1 As shown, the composite alumina preparation method comprises the following steps:

[0041] Step S1, weighing flaky aluminum oxide powder with a particle size D50 of 5-35 μm and mixing it with deionized water, heating it at 60-80° C. and stirring and mixing it to fully disperse the flaky aluminum oxide powder to obtain a mixed solution A, that is, a dispersion solution.

[0042] Step S2, adding the mixed solution of iron salt and ferrous salt to the mixed solution A obtained in step S1 at a uniform speed, stirring and mixing evenly, and then slowly and uniformly adding ammonia water to adjust the pH to alkaline, preferably controlling the uniform speed of adding ammonia water until the pH of the solution reaches 12, to obtain a mixed solution B. Fe3O4 is deposited on the surface of the flaky aluminum oxide in the mixed solution B to form a black precipitate.

[0043] Ammonia water is used to adjust the pH of the solution, and the pH is adjusted to 12 to terminate the reaction, which can effectively ensure that Fe3O4 is firmly deposited and attached to the surface of the flaky alumina, and the deposition is complete, so that the obtained composite alumina has good stability.

[0044] Step S3, filtering, washing and drying the precipitate in the mixed solution B obtained in step S2 to obtain composite alumina powder. The composite alumina powder is a flaky alumina surface coated with a thin layer of Fe3O4, and the composite alumina powder can be expressed as Fe3O4-Al2O3.

[0045] Preferably, in step S1, flaky alumina with a particle size D50 of 5 to 35 μm is selected as a raw material to prepare composite alumina.

[0046] The flaky aluminum oxide powder can be prepared by the following method, which comprises the following steps:

[0047] Step P1, weigh boehmite powder and add it into a composite molten salt aqueous solution of Na2SO4 and K2SO4, stir to evenly disperse the boehmite, and obtain a mixed solution C.

[0048] Step P2, adding trisodium phosphate and titanyl sulfate to the evenly dispersed mixed solution C, stirring until completely dissolved, to obtain a mixed solution D.

[0049] Step P3, drying the mixed solution D obtained in step P2, and the dried powder enters a high-temperature furnace for sintering. After the sintered block is cooled to room temperature, it is washed and dried to obtain flaky alumina powder.

[0050] Preferably, the mass ratio of boehmite to the mass ratio of the composite molten salt (Na2SO4 and K2SO4) is controlled to be 1:4; the mass ratio of Na2SO4 and K2SO4 in the composite molten salt is 1:1; and the mass concentration of the molten salt in the composite molten salt aqueous solution prepared by Na2SO4 and K2SO4 is 300 g / L. Thus, a mixed solution C is prepared.

[0051] Furthermore, it is preferred that the amount of trisodium phosphate added in step P2 is controlled to be 2.5% of the mass of the boehmite powder weighed in step P1, and the amount of titanyl sulfate added is controlled to be 4% of the mass of the boehmite powder weighed in step P1.

[0052] By adopting the flaky alumina preparation method and controlling the addition steps and addition amounts of boehmite, composite molten salt, trisodium phosphate and titanyl sulfate, it can be effectively ensured that flaky alumina powder with uniform particle size, particle size D50 in the range of 5-35 μm and moderate thickness is obtained, thereby providing raw materials that meet the requirements for the subsequent preparation of composite alumina.

[0053] In step S2, regarding the mixed solution of ferric salt and ferrous salt, the molar ratio of ferric salt to ferrous salt is preferably controlled to be 2:1, and the concentration of iron ions in the mixed solution is about 0.5 mol / L.

[0054] Wherein, the iron salt may include one or more of iron sulfate, iron nitrate, and iron chloride;

[0055] The ferrous salt may include one or more of ferrous sulfate, ferrous nitrate, and ferrous chloride.

[0056] Preferably, the ratio of the total mass of the ferric salt and the ferrous salt to the mass of the flaky aluminum oxide weighed and added in step S1 is controlled to be 0.5-3:1.

[0057] Controlling the particle size D50 of flaky alumina to 5~35μm and the mass ratio of iron salt to flaky alumina to 0.5~3:1 can effectively ensure that the magnetic properties of the obtained composite alumina are oriented under the induction of an external magnetic field when preparing thermal conductive materials, and that the flaky powders are orderly arranged and have a larger contact area, thereby effectively improving the thermal conductivity of the thermal conductive material.

[0058] The composite alumina is preferably a flaky alumina surface coated with a thin layer of Fe3O4, the mass content of Fe3O4 in the composite alumina is in the range of 0.5-5%, and the Fe3O4 coating is in situ growth and disordered coverage, and the specific surface area of ​​the composite alumina is 4-30m 2 / g range.

[0059] The composite alumina (Fe3O4-Al2O3) obtained by the above preparation method can be applied to thermal conductive materials of electronic equipment.

[0060] When preparing thermal conductive materials for electronic equipment, the composite alumina is added as a thermal conductive medium. The filling rate of the composite alumina in the thermal conductive material is within the range of 20-60% to obtain a thermal conductivity that meets the requirements.

[0061] When the above-mentioned composite alumina is used to prepare a thermal conductive material, it is preferably subjected to an induced orientation treatment in an external vertical magnetic field before being poured into a mold for solidification, so that the flaky composite alumina can be arranged in an orderly manner and stacked parallel to each other to increase the contact thermal conductive area, thereby effectively improving the thermal conductivity of the thermal conductive material.

[0062] Preferably, the intensity of the external magnetic field is controlled to be 400 mT and the induction time is 0 to 120 min.

[0063] Furthermore, this embodiment also provides a method for preparing a thermally conductive material using the composite alumina, the method comprising the following steps:

[0064] Step T1, dicyandiamide and epoxy resin are mixed and dissolved in DMF (N,N-dimethylformamide).

[0065] Step T2, weighing composite alumina (Fe3O4-Al2O3), adding anhydrous ethanol and ternary blended organosilicone to the composite alumina, coupling reaction for a certain time, heating to 80°C after the reaction to volatilize most of the ethanol, and obtaining coupled modified composite alumina.

[0066] Step T3, mixing the coupled modified composite alumina prepared in step T2 with the mixed solution prepared in step T1, stirring and degassing under vacuum after mixing, and pouring into a mold after degassing.

[0067] Step T4, placing the mold in a vertical magnetic field formed by two horizontally placed NdFeB permanent magnets for induced orientation.

[0068] Step T5, after a period of time of induced orientation in the vertical magnetic field, heating and curing treatment are performed to obtain a thermally conductive material.

[0069] Among them, it is preferred to control the mass ratio of epoxy resin and dicyandiamide to 25:1; control the filling rate of composite alumina to be in the range of 20% to 60%; the vertical magnetic field strength formed by the NdFeB permanent magnet is 400mT, and the induced orientation time is controlled to be 0 to 120min; the parameters of the heating and curing treatment are 160°C, 5MPa hot pressing, and treatment for 20min.

[0070] Example 1

[0071] Take 30g of boehmite powder, add it to a composite molten salt aqueous solution containing 120g of Na2SO4 and K2SO4 (where the mass ratio of Na2SO4 and K2SO4 is 1:1, and the mass concentration of the molten salt in the composite molten salt aqueous solution is 300g / L), stir to make the boehmite powder disperse evenly, then add 0.75g of trisodium phosphate (accounting for 2.5% of the mass of the boehmite powder) and 1.2g of titanyl sulfate (accounting for 4% of the mass of the boehmite powder), stir until completely dissolved, and then dry the mixed solution. The powder obtained by drying is put into a high-temperature furnace for sintering. After the sintered material is cooled, it is washed and dried to obtain flaky alumina powder. Figure 2 As shown, the particles of the flaky aluminum oxide powder are flaky, with uniform particle size distribution and a particle size D50 of about 15 μm.

[0072] Weigh 20g of the prepared flaky aluminum oxide, add it to 500ml of deionized water, heat it to 60℃ and stir to disperse it, then add it to a mixed solution containing 10g of FeCl3 and FeCl2 (i.e., the total mass of iron salt and the mass ratio of flaky aluminum oxide is 0.5:1), continue stirring, and after mixing evenly, slowly add ammonia water at a uniform rate until the pH of the solution reaches 12, then stop adding ammonia water, and obtain a mixed solution with black precipitate. Filter, wash and dry the black precipitate to obtain composite aluminum oxide (Fe3O4-Al2O3) powder. Figure 3As shown, the composite alumina powder is a flaky alumina surface coated with a thin layer of Fe3O4, and the Fe3O4 coating is in-situ grown and disordered coating.

[0073] The prepared composite alumina powder is taken, coupled and modified and then mixed with a mixed solution of epoxy resin, the filling rate of the composite alumina powder is controlled to be 20%, vacuum degassed after mixing, poured into a mold, heated and cured to obtain a composite thermally conductive resin material (i.e., thermally conductive material). After testing, the thermal conductivity of the composite thermally conductive resin material is 0.68 W / mK.

[0074] Example 2

[0075] This embodiment is basically the same as the embodiment 1, except that: in the preparation of the composite thermally conductive resin material, the coupled modified composite alumina and the mixed solution of epoxy resin are mixed, vacuum degassed and poured into a mold, and then the mold and the mixed solution therein are placed in a magnetic field with an intensity of 400mT for induced orientation for 30 minutes, and then heated and cured after the magnetic field induced orientation to obtain a composite thermally conductive resin material. After testing, the thermal conductivity of the composite thermally conductive resin material is 0.77W / mK, which is about 13.24% higher than that of the composite thermally conductive resin material of the embodiment 1.

[0076] Example 3

[0077] This embodiment is basically the same as Embodiment 2, except that in the step of preparing composite alumina powder, the total mass of FeCl3 and FeCl2 added to the mixed solution of FeCl3 and FeCl2 is 20 g (ie, the total mass ratio of iron salt to flaky alumina is 1:1).

[0078] The thermal conductivity of the prepared composite thermally conductive resin material is 0.85 W / mK. Compared with the composite thermally conductive resin material of Example 2, the thermal conductivity is increased by about 10.39%.

[0079] Example 4

[0080] This embodiment is basically the same as Embodiment 2, except that in the step of preparing composite alumina powder, the total mass of FeCl3 and FeCl2 added to the mixed solution of FeCl3 and FeCl2 is 40 g (ie, the total mass ratio of iron salt to flaky alumina is 2:1).

[0081] The thermal conductivity of the prepared composite thermally conductive resin material is 0.91 W / mK. Compared with the composite thermally conductive resin material of Example 2, the thermal conductivity is increased by about 18.18%.

[0082] Example 5

[0083] This embodiment is basically the same as Embodiment 2, except that in the step of preparing composite alumina powder, the total mass of FeCl3 and FeCl2 added to the mixed solution of FeCl3 and FeCl2 is 60 g (ie, the total mass ratio of iron salt to flaky alumina is 3:1).

[0084] The thermal conductivity of the prepared composite thermally conductive resin material is 0.98 W / mK. Compared with the composite thermally conductive resin material of Example 2, the thermal conductivity is increased by about 27.27%.

[0085] As shown in Table 1, it can be deduced according to Examples 3-5 that increasing the ratio of the total mass of iron salt to the mass of flaky aluminum oxide from 0.5:1 to 3:1 can effectively improve the arrangement state of the composite aluminum oxide under the action of magnetic field induced orientation and improve the thermal conductivity of the composite thermally conductive resin material.

[0086] Example 6

[0087] This embodiment is basically the same as Embodiment 2, except that:

[0088] In the step of preparing composite alumina powder, the total mass of FeCl3 and FeCl2 in the mixed solution of FeCl3 and FeCl2 added is 60g (i.e., the total mass ratio of iron salt to flaky alumina is 3:1);

[0089] In the process of preparing the composite thermal conductive resin material, the induced orientation time in the magnetic field is 60 minutes.

[0090] The thermal conductivity of the prepared composite thermally conductive resin material is 1.1 W / mK, which is about 12.24% higher than that of the composite thermally conductive resin material of Example 5. It can be seen that extending the magnetic field induced orientation time from 30 min to 60 min can further optimize the arrangement of the flaky composite aluminum oxide in the composite thermally conductive resin material, thereby further improving the thermal conductivity.

[0091] Example 7

[0092] This embodiment is basically the same as Embodiment 2, except that:

[0093] In the step of preparing composite alumina powder, the total mass of FeCl3 and FeCl2 in the mixed solution of FeCl3 and FeCl2 added is 60g (i.e., the total mass ratio of iron salt to flaky alumina is 3:1);

[0094] In the process of preparing the composite thermal conductive resin material, the filling rate of the composite alumina powder is 30%, and the induced orientation time in the magnetic field is 120 minutes.

[0095] The thermal conductivity of the prepared composite thermally conductive resin material is 1.29 W / mK, which is about 67.53% higher than that of the composite thermally conductive resin material of Example 2, and about 17.27% higher than that of the composite thermally conductive resin material of Example 6.

[0096] Example 8

[0097] This embodiment is basically the same as Embodiment 2, except that:

[0098] In the step of preparing composite alumina powder, the total mass of FeCl3 and FeCl2 in the mixed solution of FeCl3 and FeCl2 added is 60g (i.e., the total mass ratio of iron salt to flaky alumina is 3:1);

[0099] In the process of preparing the composite thermal conductive resin material, the filling rate of the composite alumina powder is 40%, and the induced orientation time in the magnetic field is 120 minutes.

[0100] The thermal conductivity of the prepared composite thermally conductive resin material is 1.36 W / mK. Compared with the composite thermally conductive resin material of Example 7, the thermal conductivity is increased by about 5.43%.

[0101] Example 9

[0102] This embodiment is basically the same as Embodiment 2, except that:

[0103] In the step of preparing composite alumina powder, the total mass of FeCl3 and FeCl2 in the mixed solution of FeCl3 and FeCl2 added is 60g (i.e., the total mass ratio of iron salt to flaky alumina is 3:1);

[0104] In the process of preparing the composite thermal conductive resin material, the filling rate of the composite alumina powder is 50%, and the induced orientation time in the magnetic field is 120 minutes.

[0105] The thermal conductivity of the prepared composite thermally conductive resin material is 1.49 W / mK. Compared with the composite thermally conductive resin material of Example 7, the thermal conductivity is increased by about 15.50%; compared with the composite thermally conductive resin material of Example 8, the thermal conductivity is increased by about 9.59%.

[0106] Example 10

[0107] This embodiment is basically the same as Embodiment 2, except that:

[0108] In the step of preparing composite alumina powder, the total mass of FeCl3 and FeCl2 in the mixed solution of FeCl3 and FeCl2 added is 60g (i.e., the total mass ratio of iron salt to flaky alumina is 3:1);

[0109] In the process of preparing the composite thermal conductive resin material, the filling rate of the composite alumina powder is 60%, and the induced orientation time in the magnetic field is 120 minutes.

[0110] The thermal conductivity of the prepared composite thermally conductive resin material is 1.55 W / mK. Compared with the composite thermally conductive resin material of Example 7, the thermal conductivity is increased by about 20.16%; compared with the composite thermally conductive resin material of Example 9, the thermal conductivity is increased by about 4.03%.

[0111] As shown in Table 1, it can be deduced from Examples 7-10 that as the filling rate of composite alumina (30-60%) increases, the thermal conductivity of the composite thermally conductive resin material can be further improved.

[0112] Table 1 is a summary table of important index parameters in Examples 1-10

[0113] According to the data of Example 1 in Table 1, when the composite alumina powder filling rate is as low as 20% and no magnetic field induced orientation treatment is performed, the obtained composite thermally conductive resin material still has a relatively high thermal conductivity (0.68W / mK), indicating that the composite alumina of the present application can effectively improve the thermal conductivity of the organic matrix when used as a thermal conductive medium to fill and prepare thermally conductive materials. The reason for this is that the Fe3O4 attached to the surface of the composite alumina makes the flaky composite alumina magnetic. When filling and preparing thermally conductive materials, the flaky powders can be adsorbed and stacked to a certain extent through mutual magnetic adsorption, thereby increasing the contact area and improving the thermal conductivity.

[0114] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing composite alumina, characterized in that: The steps include: S1, mixing flaky aluminum oxide powder with deionized water, heating, stirring and dispersing, to obtain a mixed solution A; S2, adding a mixed solution of ferric salt and ferrous salt to the mixed solution A, mixing evenly, and then slowly adding ammonia water to adjust the pH to alkaline, to obtain a mixed solution B; S3, filtering, washing and drying the precipitate in the mixed solution B to obtain composite alumina powder.

2. The method for preparing composite alumina according to claim 1, characterized in that: The particle size D50 of the flaky aluminum oxide is 5-35 μm.

3. The method for preparing composite alumina according to claim 1 or 2, characterized in that: The preparation method of the flaky aluminum oxide comprises the following steps: P1, add boehmite powder into a composite molten salt aqueous solution of Na2SO4 and K2SO4, disperse evenly, and obtain a mixed solution C; P2, adding trisodium phosphate and titanyl sulfate to the mixed solution C, stirring until completely dissolved, to obtain a mixed solution D; P3, drying the mixed solution D, sintering, washing and drying the powder to obtain the flaky aluminum oxide.

4. The method for preparing composite alumina according to claim 3, characterized in that: The mass ratio of the boehmite to the composite molten salt is 1:4; And / or, the mass ratio of Na2SO4 to K2SO4 is 1:1; And / or, the molten salt mass concentration of the composite molten salt aqueous solution is 300 g / L; And / or, the amount of trisodium phosphate added is 2.5% of the mass of the boehmite powder, and the amount of titanyl sulfate added is 4% of the mass of the boehmite powder.

5. The method for preparing composite alumina according to claim 1, characterized in that: The iron salt includes one or more of ferric sulfate, ferric nitrate and ferric chloride; And / or, the ferrous salt includes one or more of ferrous sulfate, ferrous nitrate, and ferrous chloride; And / or, in the mixed solution of the ferric salt and the ferrous salt, the concentration of the iron ion is 0.5 mol / L, and the molar ratio of the ferric salt to the ferrous salt is 2:1; And / or, the ratio of the total mass of the ferric salt and the ferrous salt to the mass of the flaky aluminum oxide is 0.5-3:

1.

6. The method for preparing composite alumina according to claim 1, characterized in that: In step S2, aqueous ammonia is added to adjust the pH to 12 to obtain a mixed solution B.

7. A composite alumina, characterized in that: The composite alumina is prepared by the composite alumina preparation method according to any one of claims 1 to 6.

8. A composite alumina, characterized in that: The composite alumina is a flaky alumina surface coated with a thin layer of Fe3O4, the mass content of Fe3O4 in the composite alumina is 0.5-5%; the specific surface area of ​​the composite alumina is 4-30m 2 / g.

9. The use of the composite alumina according to claim 7 or 8, characterized in that: This includes application of the composite alumina in thermal conductive materials for electronic equipment.

10. The use of the composite alumina according to claim 9, characterized in that: The filling rate of the composite alumina in the thermal conductive material is 20-60%; And / or, during the preparation of the thermal conductive material, an external vertical magnetic field is applied to induce orientation treatment, the magnetic field strength is 400 mT, and the induction time is 0 to 120 min.

Citation Information

Cited By

  • Jade cool fiber and preparation method thereof