Recycled concrete preparation process

By calcining, grinding and vacuum impregnation of waste concrete, combined with nano silica and high-performance additives, the compressive strength and durability of recycled concrete are improved, and the compressive strength reduction caused by the high substitution rate of recycled aggregates is solved. , realize the efficient reuse of waste concrete resources.

CN119059774APending Publication Date: 2024-12-03CHONGQING XINKE NEW BUILDING MATERIALS CO LTD

Patent Information

Application Number
CN202411211885.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The compressive strength of recycled concrete will decrease with the increase in the replacement rate of recycled aggregate, resulting in its use rate lower than expected.

Method used

By coarsely crushing, removing impurities, calcining and grinding of waste concrete, combining vacuum impregnation technology and the use of nano-silica, we accurately proportion a variety of high-performance additives to improve the bonding strength and interface bonding between aggregate and cement slurry and the bonding force of the bonding force between aggregate and cement slurry , reduce water absorption.

Benefits of technology

The compressive strength, permeability and durability of recycled concrete are significantly improved, the problem of reduced compressive strength is solved, and efficient reuse of waste concrete resources is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020515740000081
    Figure BDA0005020515740000081
  • Figure BDA0005020515740000091
    Figure BDA0005020515740000091
Patent Text Reader

Abstract

The invention relates to the field of environment-friendly concrete, and particularly discloses a preparation process of recycled concrete. The preparation process of the recycled concrete comprises the following steps: carrying out coarse crushing on collected waste concrete blocks, removing impurities, carrying out secondary crushing, cleaning, screening waste concrete particles with the particle size of 4-10mm as recycled coarse aggregates, taking waste concrete particles with the particle size of 1-3mm as recycled fine aggregates, and carrying out secondary crushing on the recycled fine aggregates to obtain recycled concrete; calcining the screened recycled coarse aggregate and recycled fine aggregate in roasting equipment, and respectively grinding the calcined recycled coarse aggregate and recycled fine aggregate; uniformly mixing the recycled coarse aggregate, the recycled fine aggregate, cement, fly ash, silica fume, a water reducing agent, an air entraining agent and water to obtain the recycled concrete. The preparation process of the recycled concrete solves the problem that the compressive strength of the recycled concrete is reduced along with the increase of the replacement rate of the recycled aggregate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of environmentally friendly concrete, and more specifically, to a process for preparing recycled concrete. Background Art

[0002] With the continuous development of the global economy and the acceleration of urbanization, the demand for concrete has increased dramatically. According to statistics, the annual output of concrete in the world is about 2.8 billion cubic meters, and my country, as a major concrete producer and consumer, accounts for about 45% of the world's total annual output. However, behind this huge output, there are serious resource and environmental problems.

[0003] The main components of concrete include cement, water and aggregates, of which aggregates account for about 75% of the total concrete. Natural aggregates, such as sand and gravel, are non-renewable resources, and their formation requires a long geological period. In the past, due to the weak awareness of resource and environmental protection, people generally believed that sand and gravel were cheap and widespread, so they were mined on a large scale, even abused, resulting in a sharp decrease in natural sand and gravel resources and serious damage to the natural ecological environment. In the long run, natural aggregates will face a serious shortage problem.

[0004] On the other hand, with the advancement of urbanization, a large number of old buildings have been demolished, generating a huge amount of construction waste. According to statistics, my country produces 160 million tons of waste concrete each year, and it increases at an average annual rate of 8%. These construction wastes not only occupy a large amount of land resources, but the traditional landfill or stacking treatment methods will further aggravate the tension of land resources. At the same time, the dust generated during the demolition process also causes serious pollution to the environment.

[0005] In the face of the above challenges, recycled concrete has emerged as an innovative building material. The production process of this concrete not only solves the problem of waste concrete disposal, but also reduces the amount of natural aggregate mining, which is of great significance to alleviating resource shortages and ecological environmental damage. However, due to the large porosity of recycled aggregates, the water absorption rate also increases, making the compressive strength of recycled concrete decrease with the increase of recycled aggregate replacement rate. Therefore, the current utilization rate of recycled concrete remains at a low level. Summary of the invention

[0006] In order to solve the problem that the compressive strength of recycled concrete decreases with the increase of recycled aggregate replacement rate, the present application provides a recycled concrete preparation process.

[0007] The present application provides a recycled concrete preparation process using the following technical solutions: A recycled concrete preparation process comprises the following steps: The collected waste concrete blocks are roughly crushed and impurities are removed, and then the roughly crushed waste concrete blocks are crushed for the second time, and the waste concrete particles after the second crushing are cleaned, impurities attached to the surface are removed, and dehydration treatment is performed; waste concrete particles with a particle size of 4-10mm are screened as recycled coarse aggregate, and waste concrete particles with a particle size of 1-3mm are used as recycled fine aggregate; The screened recycled coarse aggregate and recycled fine aggregate are placed in a roasting device and calcined at 700-750°C for 1-3h; Grinding the calcined recycled coarse aggregate and recycled fine aggregate separately; The recycled concrete is obtained by uniformly mixing 600-1000 parts of recycled coarse aggregate, 500-800 parts of recycled fine aggregate, 300-400 parts of cement, 50-150 parts of fly ash, 10-50 parts of silica fume, 5-15 parts of water reducer, 1-5 parts of air entraining agent and 150-200 parts of water in parts by weight.

[0008] By adopting the above technical solution, the waste concrete blocks are roughly crushed, impurities are removed, secondary crushed, cleaned and dehydrated, and the soil, oil and other unfavorable impurities attached to the surface of the aggregate are effectively removed, the surface state of the aggregate is improved, and the bonding strength between the aggregate and the cement paste is improved. The screened recycled aggregate is calcined at 700-750℃. This process can remove the residual moisture and some organic matter in the aggregate, and activate the recycled aggregate at the same time. The calcined aggregate is ground to further refine its particle surface, which is conducive to forming a stronger interface bonding force. The combination of calcination and grinding can further reduce the proportion of cement mortar mixed in the recycled aggregate, realize the separation of aggregate and cement paste, and thus reduce the water absorption rate of the recycled aggregate. By precisely controlling the proportions of raw materials such as recycled coarse aggregate, recycled fine aggregate, cement, fly ash, silica fume, water reducer, air entraining agent and water, and fully mixing them evenly, not only the working performance of concrete is guaranteed, but also the comprehensive properties of concrete such as compressive strength, impermeability and durability are further improved through the micro-aggregate effect, volcanic ash effect of fly ash and silica fume and the chemical action of water reducer and air entraining agent.

[0009] Optionally, the ground recycled coarse aggregate is further processed as follows: Mix epoxy resin and ethanol in a mass ratio of 10:(2-4), stir well to form an epoxy resin solution; Wash and dry the recycled coarse aggregate and place it in a vacuum impregnation device. Vacuum it to (-0.06)-(-0.08) MPa and keep it for 10-20 minutes. Then inject the epoxy resin solution into the vacuum impregnation device to ensure that the aggregate is completely immersed in the solution. Maintain the vacuum state for 30-60 minutes, slowly restore normal pressure, and keep the aggregate immersed in the solution for an additional 30 minutes. The impregnated recycled coarse aggregate is taken out and placed in an oven to dry at 60-80°C for 12-24 hours.

[0010] Optionally, nano silicon dioxide is further added to the epoxy resin solution, and the amount of the nano silicon dioxide added is 1-5% of the weight of the epoxy resin.

[0011] By adopting the above technical solution, the recycled coarse aggregate is placed in a vacuum impregnation device for treatment, and vacuuming can effectively remove moisture and air inside and on the surface of the aggregate. The epoxy resin solution impregnates the recycled coarse aggregate under a vacuum environment to ensure that the epoxy resin can penetrate into the fine pores of the aggregate. During the drying and curing process, the epoxy resin forms a dense protective layer, which effectively seals the pores of the aggregate and greatly reduces its water absorption rate. In addition, the epoxy resin has high adhesion and toughness, which can improve the physical and chemical properties of the surface of the recycled aggregate, so that it forms a stronger interface bond with the cement paste, thereby improving the overall strength of the recycled concrete. The introduction of nano-silica particles not only fills the tiny gaps inside the epoxy resin, but also forms a tighter bond at the interface between the aggregate and the epoxy resin, which is conducive to enhancing the compressive strength of the recycled concrete and solving the problem that the compressive strength of the recycled concrete will decrease with the increase of the replacement rate of the recycled aggregate.

[0012] Optionally, the ground recycled fine aggregate is further processed as follows: Clean the recycled fine aggregate and dry it to ensure that there is no moisture on its surface; The organic silicone resin and toluene are mixed in a weight ratio of 1:(1-1.5) to obtain a mixed liquid, and then 1-10% of the mass of the mixed liquid is added with a silane coupling agent, and the mixture is stirred thoroughly to obtain an organic silicone resin solution; Immerse the recycled fine aggregate in the silicone resin solution, keep it at 40-60℃ for 3-5h, and continue to stir at a low speed of 20-40r / min; After the insulation is completed, the recycled fine aggregate is placed in an oven and dried and cured at 60-80°C for 2-4 hours.

[0013] By adopting the above technical solution, toluene as a solvent can effectively reduce the viscosity of silicone resin, making it easier to penetrate into the pores of fine aggregate. Silane coupling agent can enhance the bonding force between silicone resin and recycled fine aggregate and improve the treatment effect. The recycled fine aggregate is immersed in the silicone resin solution, and the temperature and stirring are controlled to ensure that the silicone resin can fully penetrate into the interior and surface of the fine aggregate to form a uniform coating. The curing process of the silicone resin is promoted by heating, so that it is firmly attached to the surface of the aggregate to form a dense protective film. This protective film can significantly reduce the water absorption rate of fine aggregate, thereby solving the problem that the compressive strength of recycled concrete will decrease with the increase of the replacement rate of recycled aggregate.

[0014] Optionally, the calcined recycled coarse aggregate and recycled fine aggregate are ground separately and then subjected to the following treatments: The fine powder is collected and ground, and the fine powder is subjected to high-energy ball milling to obtain recycled micro powder with a particle size distribution of 0.01-0.05 mm. The recycled micro powder is mixed with cement, and the recycled micro powder accounts for 20-30% of the cement used in the recycled concrete.

[0015] By adopting the above technical solution, the recycled micropowder has a certain volcanic ash activity, and high-energy ball milling can further refine the particles, making the recycled micropowder have a more uniform particle size distribution and higher activity, and can react with cement hydration products to generate more CSH gel, which helps to improve the microstructure of concrete and make it denser and stronger. Mixing recycled micropowder with cement and using recycled micropowder to replace part of the cement without reducing the workability of concrete not only reduces dependence on natural resources, but also reduces carbon dioxide emissions generated during cement production, which has significant environmental benefits.

[0016] Optionally, the regenerated micro powder is further processed as follows: The regenerated micro powder obtained by high-energy ball milling is immersed in a sodium silicate solution with a mass concentration of 10-15%, and after immersing for 2-4 hours, the regenerated micro powder is taken out and dried.

[0017] By adopting the above technical solution, a highly active silicate film is formed on the surface of the recycled micropowder through the treatment of sodium silicate solution. This protective film can not only improve the chemical reaction activity of the recycled micropowder, but also enhance its interfacial bonding performance with the cement matrix. Due to the presence of the silicate film, the micropowder can be more evenly distributed in the cement matrix, with a better filling effect. The recycled micropowder treated with sodium silicate solution can better combine with the cement paste, significantly improving the compressive strength, crack resistance and durability of the recycled concrete, solving the problem of performance degradation of recycled concrete at a high replacement rate.

[0018] Optionally, the water reducing agent includes sulfonated naphthalene formaldehyde condensate and nano calcium titanate, and the sulfonated naphthalene formaldehyde condensate and nano calcium titanate are mixed in a mass ratio of 10:(1-2).

[0019] By adopting the above technical solution, the combination of SNF and nano calcium titanate, SNF can significantly improve the fluidity of recycled concrete, making it easier to pour and shape. The filling effect of nano calcium titanate and the enhanced interfacial bonding performance also help to improve the overall strength. The water-reducing effect of SNF and the filling effect of nano calcium titanate work together to reduce the porosity and microcracks in the concrete, reducing the risk of shrinkage deformation and cracks in the concrete.

[0020] Optionally, the air entraining agent includes, by mass percentage, 50-60% sodium alkylbenzene sulfonate, 10-20% sodium rosin acid, 10-15% sodium stearate, 5-10% ethylene glycol, and 5-10% water.

[0021] By adopting the above technical solution, sodium alkylbenzene sulfonate promotes the formation and stability of bubbles by reducing the surface tension of cement paste. Sodium rosin acid provides an air entraining effect, enhances the stability of bubbles, and makes them less likely to break during concrete mixing and hardening. Sodium stearate increases the durability of bubbles and improves the uniform distribution of bubbles, thereby improving the frost resistance and durability of concrete. Ethylene glycol acts as a solvent and plasticizer to improve the working performance of the mixture and make the air entraining agent more evenly distributed in the concrete.

[0022] In summary, this application has the following beneficial effects: 1. This application effectively removes impurities in waste concrete and activates aggregates through refined crushing, cleaning, screening, calcining and grinding steps, realizes the separation of aggregates and cement slurry, thereby reducing the water absorption rate of recycled aggregates, and then accurately proportions and mixes a variety of high-performance additives, which not only optimizes the surface state of aggregates, but also significantly improves the compressive strength, impermeability and durability of recycled concrete, thereby realizing the efficient reuse of waste concrete resources.

[0023] 2. In this application, it is preferred to treat the recycled coarse aggregate in an epoxy resin solution by vacuum impregnation technology, effectively remove moisture and air, allow the epoxy resin to penetrate into the pores, form a dense protective layer, significantly reduce water absorption and enhance adhesion and toughness. Combined with nano-silicon dioxide particles, the voids are further filled and the interface bonding is strengthened, effectively improving the compressive strength and overall performance of the recycled concrete, and solving the problem of reduced strength under high replacement rate of recycled aggregate.

[0024] 3. In this application, it is preferred to use toluene as a solvent to reduce the viscosity of the silicone resin, and to combine with a silane coupling agent to enhance the bonding force, immerse the recycled fine aggregate in the resin solution, and ensure full penetration through temperature control and stirring to form a uniform coating layer. Subsequently, heat and cure to make the resin tightly adhere to the surface of the aggregate, build a dense protective film, significantly reduce water absorption, and effectively alleviate the problem of decreased compressive strength of recycled concrete caused by the high replacement rate of recycled aggregate. DETAILED DESCRIPTION

[0025] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources. Example

[0026] Example 1 A recycled concrete preparation process: The collected waste concrete blocks are put into a crusher for coarse crushing, the waste concrete blocks after coarse crushing are screened to remove impurities such as steel bars and plastics, and then the waste concrete blocks after coarse crushing are crushed for a second time, and the waste concrete particles after the second crushing are cleaned to remove impurities attached to the surface and dehydrated; Screening waste concrete particles with a particle size of 4-10 mm as recycled coarse aggregate, and waste concrete particles with a particle size of 1-3 mm as recycled fine aggregate; The screened recycled coarse aggregate and recycled fine aggregate were placed in a roasting furnace and calcined at 730°C for 2h; The calcined recycled coarse aggregate and recycled fine aggregate are put into a grinder for grinding respectively; 80 kg of recycled coarse aggregate, 60 kg of recycled fine aggregate, 35 kg of 42.5R silicate cement, 10 kg of grade II fly ash, 3 kg of grade I silica fume, 1 kg of Shanghai Yunzhe New Materials FDN-C naphthalene-based water reducer, 0.3 kg of Henan Jingcan Chemical SY-5 triterpenoid saponin air entraining agent and 18 kg of water were mixed evenly in a concrete mixer to obtain recycled concrete.

[0027] Example 2 A recycled concrete preparation process, which is different from Example 1 in that: 60 kg of recycled coarse aggregate, 50 kg of recycled fine aggregate, 30 kg of 42.5R silicate cement, 5 kg of Class II fly ash, 1 kg of Class I silica fume, 0.5 kg of Shanghai Yunzhe New Materials FDN-C naphthalene-based water reducer, 0.1 kg of Henan Jingcan Chemical SY-5 triterpene saponin air entraining agent and 15 kg of water are mixed evenly in a concrete mixer to obtain recycled concrete.

[0028] Example 3 A recycled concrete preparation process, which is different from Example 1 in that: 100 kg of recycled coarse aggregate, 80 kg of recycled fine aggregate, 40 kg of 42.5R silicate cement, 15 kg of Class II fly ash, 5 kg of Class I silica fume, 1.5 kg of Shanghai Yunzhe New Materials FDN-C naphthalene-based water reducer, 0.5 kg of Henan Jingcan Chemical SY-5 triterpene saponin air entraining agent and 20 kg of water are mixed evenly in a concrete mixer to obtain recycled concrete.

[0029] Example 4 A recycled concrete preparation process: The collected waste concrete blocks are put into a crusher for coarse crushing, the waste concrete blocks after coarse crushing are screened to remove impurities such as steel bars and plastics, and then the waste concrete blocks after coarse crushing are crushed for a second time, and the waste concrete particles after the second crushing are cleaned to remove impurities attached to the surface and dehydrated; Screening waste concrete particles with a particle size of 4-10 mm as recycled coarse aggregate, and waste concrete particles with a particle size of 1-3 mm as recycled fine aggregate; The screened recycled coarse aggregate and recycled fine aggregate were placed in a roasting furnace and calcined at 730°C for 2h; The calcined recycled coarse aggregate and recycled fine aggregate are put into a grinder for grinding respectively; Epoxy resin and ethanol are mixed in a mass ratio of 10:3, and stirred thoroughly to form an epoxy resin solution. The recycled coarse aggregate is washed and dried, and then placed in a vacuum impregnation device, and evacuated to -0.07MPa, and maintained for 15 minutes. The epoxy resin solution is then injected into the vacuum impregnation device to ensure that the recycled coarse aggregate is completely immersed in the solution. The vacuum state is maintained for 40 minutes, and normal pressure is slowly restored. The aggregate is kept immersed in the solution for an additional 30 minutes. The impregnated recycled coarse aggregate is taken out and placed in an oven for drying at 70°C for 18 hours. 80 kg of recycled coarse aggregate, 60 kg of recycled fine aggregate, 35 kg of 42.5R silicate cement, 10 kg of grade II fly ash, 3 kg of grade I silica fume, 1 kg of Shanghai Yunzhe New Materials FDN-C naphthalene-based water reducer, 0.3 kg of Henan Jingcan Chemical SY-5 triterpenoid saponin air entraining agent and 18 kg of water were mixed evenly in a concrete mixer to obtain recycled concrete.

[0030] Example 5 A recycled concrete preparation process: The collected waste concrete blocks are put into a crusher for coarse crushing, the waste concrete blocks after coarse crushing are screened to remove impurities such as steel bars and plastics, and then the waste concrete blocks after coarse crushing are crushed for a second time, and the waste concrete particles after the second crushing are cleaned to remove impurities attached to the surface and dehydrated; Screening waste concrete particles with a particle size of 4-10 mm as recycled coarse aggregate, and waste concrete particles with a particle size of 1-3 mm as recycled fine aggregate; The screened recycled coarse aggregate and recycled fine aggregate were placed in a roasting furnace and calcined at 730°C for 2h; The calcined recycled coarse aggregate and recycled fine aggregate are put into a grinder for grinding respectively; Epoxy resin and ethanol are mixed in a mass ratio of 10:3, and stirred thoroughly to form an epoxy resin solution. Nano-silicon dioxide accounting for 3% of the weight of the epoxy resin is then added to the epoxy resin solution. The recycled coarse aggregate is washed and dried and placed in a vacuum impregnation device, and vacuumed to -0.07MPa for 15 minutes. The epoxy resin solution is then injected into the vacuum impregnation device to ensure that the recycled coarse aggregate is completely immersed in the solution. The vacuum state is maintained for 40 minutes, and normal pressure is slowly restored. The aggregate is kept immersed in the solution for an additional 30 minutes. The impregnated recycled coarse aggregate is taken out and placed in an oven for drying at 70°C for 18 hours. 80 kg of recycled coarse aggregate, 60 kg of recycled fine aggregate, 35 kg of 42.5R silicate cement, 10 kg of grade II fly ash, 3 kg of grade I silica fume, 1 kg of Shanghai Yunzhe New Materials FDN-C naphthalene-based water reducer, 0.3 kg of Henan Jingcan Chemical SY-5 triterpenoid saponin air entraining agent and 18 kg of water were mixed evenly in a concrete mixer to obtain recycled concrete.

[0031] Example 6 A recycled concrete preparation process: The collected waste concrete blocks are put into a crusher for coarse crushing, the waste concrete blocks after coarse crushing are screened to remove impurities such as steel bars and plastics, and then the waste concrete blocks after coarse crushing are crushed for a second time, and the waste concrete particles after the second crushing are cleaned to remove impurities attached to the surface and dehydrated; Screening waste concrete particles with a particle size of 4-10 mm as recycled coarse aggregate, and waste concrete particles with a particle size of 1-3 mm as recycled fine aggregate; The screened recycled coarse aggregate and recycled fine aggregate were placed in a roasting furnace and calcined at 730°C for 2h; The calcined recycled coarse aggregate and recycled fine aggregate are put into a grinder for grinding respectively; The recycled fine aggregate is cleaned and dried to ensure that there is no moisture on its surface. The silicone resin and toluene are mixed in a weight ratio of 1:1.2 to obtain a mixed solution, and then 5% of the mass of the mixed solution is added with a silane coupling agent, and the mixture is fully stirred to obtain a silicone resin solution. The recycled fine aggregate is immersed in the silicone resin solution, and the mixture is kept warm at 50°C for 4 hours, and the mixture is continuously stirred at a low speed of 30 r / min. After the insulation is completed, the recycled fine aggregate is placed in an oven and dried and cured at 70°C for 3 hours; 80 kg of recycled coarse aggregate, 60 kg of recycled fine aggregate, 35 kg of 42.5R silicate cement, 10 kg of grade II fly ash, 3 kg of grade I silica fume, 1 kg of Shanghai Yunzhe New Materials FDN-C naphthalene-based water reducer, 0.3 kg of Henan Jingcan Chemical SY-5 triterpenoid saponin air entraining agent and 18 kg of water were mixed evenly in a concrete mixer to obtain recycled concrete.

[0032] Example 7 A recycled concrete preparation process: The collected waste concrete blocks are put into a crusher for coarse crushing, the waste concrete blocks after coarse crushing are screened to remove impurities such as steel bars and plastics, and then the waste concrete blocks after coarse crushing are crushed for a second time, and the waste concrete particles after the second crushing are cleaned to remove impurities attached to the surface and dehydrated; Screening waste concrete particles with a particle size of 4-10 mm as recycled coarse aggregate, and waste concrete particles with a particle size of 1-3 mm as recycled fine aggregate; The screened recycled coarse aggregate and recycled fine aggregate were placed in a roasting furnace and calcined at 730°C for 2h; The calcined recycled coarse aggregate and recycled fine aggregate are put into a grinder for grinding respectively, and the fine powder is collected and ground. The fine powder is subjected to high-energy ball milling to obtain recycled micro powder with a particle size distribution of 0.01-0.05 mm, and the recycled micro powder is mixed with cement. The recycled micro powder accounts for 20-30% of the cement used in the recycled concrete; 80 kg of recycled coarse aggregate, 60 kg of recycled fine aggregate, 35 kg of 42.5R silicate cement, 8.75 kg of recycled micropowder, 10 kg of grade II fly ash, 3 kg of grade I silica fume, 1 kg of Shanghai Yunzhe New Materials FDN-C naphthalene-based water reducer, 0.3 kg of Henan Jingcan Chemical SY-5 triterpenoid saponin air entraining agent and 18 kg of water were mixed evenly in a concrete mixer to obtain recycled concrete.

[0033] Example 8 A recycled concrete preparation process, which is different from Example 7 in that: the recycled micropowder obtained by high-energy ball milling is immersed in a sodium silicate solution with a mass concentration of 12%, and after soaking for 3 hours, the recycled micropowder is taken out and dried.

[0034] Example 9 A recycled concrete preparation process, which is different from Example 1 in that the water reducing agent is a mixture of sulfonated naphthalene formaldehyde condensate and nano calcium titanate in a mass ratio of 10:1.5.

[0035] Example 10 A recycled concrete preparation process, which is different from Example 1 in that the air entraining agent is a mixture of 55% sodium alkylbenzene sulfonate, 15% sodium rosin acid, 12% sodium stearate, 8% ethylene glycol, and 10% water by mass percentage.

[0036] Comparative Example Comparative Example 1 A recycled concrete preparation process, which is different from Example 1 in that: the recycled coarse aggregate and the recycled fine aggregate are not calcined.

[0037] Comparative Example 2 A recycled concrete preparation process, which is different from Example 1 in that the calcined recycled coarse aggregate and recycled fine aggregate are not ground.

[0038] Comparative Example 3 A recycled concrete preparation process, which is different from Example 9 in that: no nano calcium titanate is added to the water reducing agent.

[0039] Performance testing Detection Methods According to the specific steps and requirements of the concrete compressive strength test specified in the Standard for Test Methods for Mechanical Properties of Ordinary Concrete (GB / T 50081-2019), the compressive strength of Examples 1-10 and Comparative Examples 1-3 was tested after curing for 7 days and 28 days, respectively.

[0040] Table 1 Compressive strength test It can be seen from Example 1 and Comparative Examples 1-2 and Table 1 that the screened recycled aggregate is calcined at 700-750° C. This process can remove residual moisture and some organic matter in the aggregate, and activate the recycled aggregate at the same time. The calcined aggregate is ground to further refine its particle surface, which is conducive to forming a stronger interface bonding force. In addition, through the combination of calcination and grinding, the proportion of cement mortar mixed in the recycled aggregate is further reduced, and the separation of aggregate and cement slurry is achieved, thereby reducing the water absorption rate of the recycled aggregate.

[0041] Combining Example 9 and Comparative Example 3 with Table 1, it can be seen that the filling effect of nano-calcium titanate and the enhanced interface bonding performance also help to improve the overall strength. The water-reducing effect of SNF and the filling effect of nano-calcium titanate work together to reduce the porosity and microcracks in the concrete and improve the compressive strength of the recycled concrete.

[0042] It can be seen from Examples 1-3 and Table 1 that the material ratios of the recycled concrete in Examples 1-3 of the present application can all achieve excellent compressive strength, among which the ratio in Example 1 is the best.

[0043] It can be seen from Example 1 and Example 4-5 and Table 1 that the epoxy resin solution is impregnated into the recycled coarse aggregate under a vacuum environment to ensure that the epoxy resin can penetrate into the fine pores of the aggregate to form a dense protective layer, effectively sealing the pores of the aggregate and greatly reducing its water absorption rate. In addition, the epoxy resin has high adhesion and toughness, which can improve the physical and chemical properties of the surface of the recycled aggregate, so that it forms a stronger interface bond with the cement paste, thereby improving the overall strength of the recycled concrete. The introduction of nano-silicon dioxide particles not only fills the tiny gaps inside the epoxy resin, but also forms a tighter bond at the interface between the aggregate and the epoxy resin, which is conducive to enhancing the compressive strength of the recycled concrete and solving the problem that the compressive strength of the recycled concrete will decrease with the increase of the replacement rate of the recycled aggregate.

[0044] It can be seen from Example 1 and Example 6 and Table 1 that the recycled fine aggregate is immersed in the silicone resin solution, and the temperature and stirring are controlled to ensure that the silicone resin can fully penetrate into the interior and surface of the fine aggregate to form a uniform coating layer. The curing process of the silicone resin is promoted by heating, so that it is firmly attached to the surface of the aggregate to form a dense protective film. This protective film can significantly reduce the water absorption rate of the fine aggregate, thereby solving the problem that the compressive strength of the recycled concrete will decrease with the increase of the recycled aggregate replacement rate.

[0045] Combining Example 1 and Example 7-8 with Table 1, it can be seen that the regenerated micropowder has a certain volcanic ash activity, and high-energy ball milling can further refine the particles, so that the regenerated micropowder has a more uniform particle size distribution and higher activity, and can react with cement hydration products to generate more CSH gel, which helps to improve the microstructure of concrete and make it more dense and strong. The regenerated micropowder treated with sodium silicate solution can better combine with cement paste and significantly improve the compressive strength of recycled concrete.

[0046] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A process for preparing recycled concrete, characterized in that: The following steps are involved: The collected waste concrete blocks are roughly crushed and impurities are removed, and then the roughly crushed waste concrete blocks are secondarily crushed, and the waste concrete particles after the second crushing are cleaned, impurities attached to the surface are removed, and dehydration treatment is performed; Screening waste concrete particles with a particle size of 4-10 mm as recycled coarse aggregate, and waste concrete particles with a particle size of 1-3 mm as recycled fine aggregate; The screened recycled coarse aggregate and recycled fine aggregate are placed in a roasting device and calcined at 700-750°C for 1-3h; Grinding the calcined recycled coarse aggregate and recycled fine aggregate separately; The recycled concrete is obtained by uniformly mixing 600-1000 parts of recycled coarse aggregate, 500-800 parts of recycled fine aggregate, 300-400 parts of cement, 50-150 parts of fly ash, 10-50 parts of silica fume, 5-15 parts of water reducer, 1-5 parts of air entraining agent and 150-200 parts of water in parts by weight.

2. The process for preparing recycled concrete according to claim 1, characterized in that: The ground recycled coarse aggregate is also subjected to the following treatments: Mix epoxy resin and ethanol in a mass ratio of 10:(2-4), stir well to form an epoxy resin solution; Wash and dry the recycled coarse aggregate and place it in a vacuum impregnation device. Vacuum it to (-0.06)-(-0.08) MPa and keep it for 10-20 minutes. Then inject the epoxy resin solution into the vacuum impregnation device to ensure that the aggregate is completely immersed in the solution. Maintain the vacuum state for 30-60 minutes, slowly restore normal pressure, and keep the aggregate immersed in the solution for an additional 30 minutes. The impregnated recycled coarse aggregate is taken out and placed in an oven to dry at 60-80°C for 12-24 hours.

3. The process for preparing recycled concrete according to claim 2, characterized in that: Nano silicon dioxide is also added to the epoxy resin solution, and the amount of the nano silicon dioxide added is 1-5% of the weight of the epoxy resin.

4. The process for preparing recycled concrete according to claim 1, characterized in that: The ground recycled fine aggregate is also processed as follows: Clean the recycled fine aggregate and dry it to ensure that there is no moisture on its surface; The organic silicone resin and toluene are mixed in a weight ratio of 1:(1-1.5) to obtain a mixed solution, and then 1-10% of the mass of the mixed solution is added with a silane coupling agent, and the mixture is stirred thoroughly to obtain an organic silicone resin solution; Immerse the recycled fine aggregate in the silicone resin solution, keep it at 40-60℃ for 3-5h, and continue to stir at a low speed of 20-40r / min; After the insulation is completed, the recycled fine aggregate is placed in an oven and dried and cured at 60-80°C for 2-4 hours.

5. The process for preparing recycled concrete according to claim 1, characterized in that: The calcined recycled coarse aggregate and recycled fine aggregate are ground and then subjected to the following treatments: The fine powder is collected and ground, and the fine powder is passed through a high-energy ball mill to obtain recycled micro powder with a particle size distribution of 0.01-0.05 mm. The recycled micro powder is mixed with cement, and the recycled micro powder accounts for 20-30% of the cement used in the recycled concrete.

6. The process for preparing recycled concrete according to claim 5, characterized in that: The regenerated micro powder is also subjected to the following treatments: The regenerated micro powder obtained by high-energy ball milling is immersed in a sodium silicate solution with a mass concentration of 10-15%. After immersion for 2-4 hours, the regenerated micro powder is taken out and dried.

7. The process for preparing recycled concrete according to claim 1, characterized in that: The water reducing agent comprises sulfonated naphthalene formaldehyde condensate and nano calcium titanate, and the sulfonated naphthalene formaldehyde condensate and the nano calcium titanate are mixed in a mass ratio of 10:(1-2).

8. The process for preparing recycled concrete according to claim 1, characterized in that: The air entraining agent comprises, by mass percentage, 50-60% sodium alkylbenzene sulfonate, 10-20% sodium rosin acid, 10-15% sodium stearate, 5-10% ethylene glycol, and 5-10% water.

Citation Information

Patent Citations

  • Green high-performance concrete and preparation method thereof

    CN112645655A

  • Corrosion-resistant recycled concrete and production process thereof

    CN112745075A

  • Preparation method of freeze-thaw resistant recycled concrete

    CN115321914A

  • Recycled concrete and preparation method thereof

    CN115925372A

  • Recycled concrete and preparation method thereof

    CN116262658A

Cited By

  • Modified recycled coarse aggregate concrete and preparation method thereof

    CN119930203A

  • Solid waste-based recycled concrete and preparation method thereof

    CN119954428A

  • A solid waste-based recycled concrete and its preparation method

    CN119954428B