High-strength degradable chitosan packaging film and preparation method thereof
By adding ingredients such as organic acids and silica to the chitosan film, a three-dimensional network structure and hydrogen bond cross-linking are formed, which solves the problems of poor mechanical properties and poor water resistance of the chitosan film, and significantly improves its tensile strength. Strength and stability, achieving high-strength, degradable packaging films.
Patent Information
- Application Number
- CN202410861613.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing chitosan membrane has poor mechanical properties and poor water resistance, making it difficult to meet the needs of industrial applications.
Use 0.2-3.5 parts of chitosan, 0.2-3.2 parts of organic acid, 0.01-0.4 parts of auxiliary film agent, 0.002-0.05 parts of emulsifier, 0.01-0.05 parts of humectant, 0.01-0.03 parts of silica, 0.01 -The composition of 0.05 parts of calcium chloride is prepared by stirring and dissolving, heating and mixing, centrifugal film formation, constant temperature drying and soaking in sodium carbonate solution to form a three-dimensional network structure and hydrogen bond cross-linking. , improve mechanical performance and stability.
It significantly improves the tensile strength and elongation at break of the chitosan film, enhances the mechanical properties and water vapor transmission rate, reduces water absorption, and ensures the uniformity and environmentally friendly biodegradability of the film.
Smart Images

Figure CN118772492A_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a high-strength degradable chitosan packaging film and a preparation method thereof, and belongs to the technical field of polymer material preparation. Background Art
[0002] Plastic is a kind of high molecular polymer artificially synthesized by polymerization or condensation with monomer as raw material. It is widely used in the field of film packaging due to its excellent mechanical properties, stable chemical properties and good processing and molding properties. However, plastic film is easy to produce gases and odors that are harmful to humans or other organisms, and have toxic effects on the human body and the environment. With the improvement of people's environmental awareness and personal health, it is an inevitable trend to use a natural polymer material to replace plastic.
[0003] Natural polymers refer to high molecular weight compounds with a linear long chain of repeating units as the basic structure, which are widely found in animals, plants and organisms. According to their functions and composition, natural polymers can be divided into: polypeptides, proteins, enzymes, polysaccharides, rubbers and resins, etc. Among them, biopolysaccharides are widely distributed in various animals and plants, so they have the advantages of wide sources, low prices and no biological toxicity. In addition, these biopolysaccharides are biodegradable, harmless and will not exist in the environment for a long time.
[0004] Chitosan is a natural polysaccharide obtained by deacetylation of chitin. Chitosan is an important component of the shells of lower plants, fungi, shrimps, crabs, insects and other crustaceans, and the cell walls of fungi. It is widely present in nature. Chitosan obtained by deacetylation of chitin also has the advantage of a wide range of sources. It is simple to prepare and has excellent properties such as non-toxicity, biodegradability and biocompatibility.
[0005] Because most chitosan molecules are amorphous, they can interact to form a dense network structure, which allows chitosan molecules to form a film with good barrier properties, making it widely used in the field of film preparation. The mechanical strength of the film plays a vital role in the application of the film, affecting the film's load-bearing capacity, service life, and safety performance. However, the existing chitosan films have poor mechanical properties, making it difficult to achieve industrial application.
[0006] In order to improve the mechanical properties of chitosan films, people have tried to modify chitosan films in various ways in order to improve their mechanical properties to meet the actual application scenarios. In view of the problem of insufficient mechanical properties of chitosan films, the commonly used modification methods are: blending modification, filling and reinforcement modification, chemical modification and surface modification. Among them, cross-linking in blending modification can effectively enhance the mechanical properties of chitosan films without affecting their degradation performance and biosafety, which is the focus of people's current research.
[0007] Some chemical crosslinking agents such as genipin, glutaraldehyde and malondialdehyde are usually used to promote the covalent bonding of polysaccharide chains in the preparation of chitosan films to ensure the uniform and stable structure of chitosan films. However, these crosslinking agents themselves have toxic and harmful properties. The biosafety of chitosan films produced by their crosslinking is questionable, which goes against the original intention of using chitosan films. Relevant studies have shown that surface carboxylic acid groups can affect each other through interactions such as electrostatics, hydrogen bonds and hydrophobic modifications, thereby changing the properties of chitosan films. Among them, polycarboxylic acids can increase the intermolecular density of chitosan films through covalent crosslinking of amide bonds formed by catalyst-free amidation reactions, thereby achieving the purpose of improving the waterproofness and oxygen barrier capacity of chitosan films. Moreover, some carboxylic acids come from natural substances such as vegetables and fruits, and are also commonly used additives in the current food field. They have shown good biosafety in various applications. The addition of these carboxylic acids will not affect the biosafety of chitosan films and are ideal modifiers. In order to fully dissolve chitosan, the organic acid added during the preparation of the film is often excessive. Studies have shown that some of the residual H + It will affect the mechanical properties and stability of the film. Soaking the initially prepared chitosan film in an alkaline solution is expected to solve this problem.
[0008] Silica is an oxide material with high specific surface area, small size, stable structure and strong mechanical strength. Existing studies have shown that silica can interact with the -OH groups in chitosan molecules to grow a three-dimensional spatial network structure. The generation of the spatial network structure can effectively enhance the tensile strength and elastic modulus of the chitosan film and reduce the water permeability of the film, but more silica doping will cause the chitosan film to become distorted. Summary of the invention
[0009] The main technical problem solved by the present invention is: in view of the problems of poor mechanical properties and poor water resistance of the existing chitosan film, a high-strength degradable chitosan packaging film and a preparation method thereof are provided.
[0010] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0011] A method for preparing a high-strength degradable chitosan packaging film. The raw materials are composed of the following by weight: 0.2-3.5 parts of chitosan, 0.2-3.2 parts of organic acid, 0.01-0.4 parts of auxiliary film agent, 0.002-0.05 parts of emulsifier, 0.01-0.05 parts of moisturizer, 0.01-0.03 parts of silicon dioxide and 0.01-0.05 parts of calcium chloride.
[0012] The preparation steps of the chitosan packaging film are:
[0013] Step 1: Weigh each raw material in order according to its composition;
[0014] Step 2: placing chitosan and deionized water in a container, stirring to fully disperse the chitosan in the deionized water, adding an organic acid to the container, heating and stirring until the chitosan is completely dissolved, to obtain a chitosan solution;
[0015] Step 3: placing the auxiliary film agent, moisturizing agent and deionized water in a container, heating and stirring to mix, and obtaining a mixed solution;
[0016] Step 4: mixing the chitosan solution with the mixed solution, heating and stirring;
[0017] Step 5: Add emulsifier, calcium chloride and silicon dioxide to the above solution, and continue stirring to obtain a film-forming solution;
[0018] Step 6: Centrifuge the film-forming solution for 5-15 minutes, remove the bubbles in the solution, cast it on the mold, dry it at a constant temperature to form a film, and cool it naturally to room temperature;
[0019] Step 7: Soak the film in a sodium carbonate solution for 0.5-5 hours;
[0020] Step 8: Spread the film horizontally and rinse it with deionized water to remove the residual sodium carbonate on the surface until the pH of the deionized water after washing is 6.5-7.5;
[0021] Step 9: After constant temperature drying to form a film, the film is naturally cooled to room temperature and peeled off to obtain a chitosan packaging film.
[0022] More preferably, the auxiliary membrane agent is one or more of acetic acid, lactic acid, ascorbic acid, citric acid, malic acid, succinic acid, adipic acid and tartaric acid.
[0023] Further preferably, the chitosan is the main material of the membrane, which is degradable and does not cause environmental pollution, and its sources include: the shells of marine arthropods such as shrimps and crabs.
[0024] Further preferably, the organic acid is one or more of acetic acid, lactic acid, ascorbic acid, citric acid, malic acid, succinic acid, adipic acid and tartaric acid;
[0025] More preferably, the auxiliary film agent is one or more of pectin, carrageenan, gelatin, agar, starch, xanthan gum, guardo gum and sodium alginate.
[0026] More preferably, the emulsifier is one or more of sucrose stearate, Tween 80, and polyvinyl pyrrolidone.
[0027] More preferably, the moisturizing agent is one or more of glycerol, 1,3-butylene glycol, 1,3-propylene glycol, polyethylene glycol, sodium carboxymethyl cellulose, sodium hyaluronate, polypropylene glycol and sorbitol.
[0028] Further preferably, in step 2, the mass ratio of chitosan to water in the chitosan aqueous solution is 1:95-1:36.
[0029] Further preferably, in step 2, the heating and stirring reaction conditions are a temperature of 30-50° C. and a time of 3-4 h.
[0030] Further preferably, in step 3, the heating and stirring reaction conditions are 30-90°C for 3-4 hours. The mass ratio of the auxiliary film agent to deionized water is 1:3000-1:400, and the mass ratio of the moisturizer to the auxiliary film agent is 1:15-5:7.
[0031] Further preferably, in step 4, the heating and stirring reaction conditions are a temperature of 30-90° C. and a time of 2-12 h.
[0032] Further preferably, in step 6, the centrifugal speed is 5000-8000 rpm, and the centrifugal time is 5-15 min.
[0033] Further preferably, in step 6, the constant temperature drying condition is a temperature of 30-60° C. and a time of 20-48 hours; and the mold is a horizontal polytetrafluoroethylene mold.
[0034] Further preferably, in step 7, the concentration range of the sodium carbonate solution is 25%-40%.
[0035] Further preferably, in step 9, the constant temperature drying condition is a temperature of 30-50° C. and a time of 0.5-18 h.
[0036] The invention discloses a high-strength degradable chitosan packaging film, wherein the chitosan packaging film has a tensile strength of 27.61-41.12 MPa and an elongation at break of 4.33-5.34%.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] (1) The technical solution of the present invention, by configuring an organic acid solvent + emulsifier system, firstly plays a good dissolving and plasticizing effect on chitosan and various raw materials added subsequently. The hydroxyl groups carried by the organic acid combine with the amino groups of chitosan to form hydrogen bonds, thereby enhancing the solubility of chitosan and other raw materials in the liquid, effectively improving the dispersion degree of the system, and ensuring the uniformity of the subsequent biofilm.
[0039] (2) The technical solution of the present invention constructs a multi-natural polysaccharide film of chitosan-auxiliary membrane agent by using an auxiliary membrane agent. After cross-linking of different polysaccharides, strong interactions such as hydrogen bonds and ionic interactions exist between molecules, which is manifested macroscopically as enhanced tensile strength and elongation at break.
[0040] (3) The technical solution of the present invention constructs a three-dimensional spatial network structure by adding silica. The network structure shows a higher density value than the original chitosan film, and a dense structure can be observed in the chitosan film modified by silica. The dense structure also affects the mechanical properties and water vapor permeability of the film. On the other hand, the full cross-linking of silica and chitosan can effectively enhance the intermolecular binding ability, so that the three-dimensional network formed by the cross-linking of chitosan and the three-dimensional network system formed by silica are interspersed and cross-linked, thereby increasing the cross-linking density of the system and further improving the mechanical properties of the system. In addition, the technical solution of the present invention also adds calcium chloride as a stabilizer. The divalent calcium ions form a three-dimensional skeleton by establishing an electrostatic effect with the anionic polymer, which increases the degree of cross-linking while effectively reducing the water absorption of the chitosan film, thereby improving its stability.
[0041] (4) The technical solution of the present invention is to soak the chitosan film obtained initially in a sodium carbonate solution to remove the residual H in the chitosan film. + The tensile stress of the soaked chitosan film was significantly increased compared with that of the unsoaked film, and with the removal of excess protons, the soaked chitosan film was easier to preserve and its stability was significantly enhanced.
[0042] (5) The chitosan and other auxiliary film agents used in the present invention are natural degradable materials. After the film is used up, it can be rapidly degraded in the environment. The final degradation products are carbon dioxide, inorganic salts and water, which can prevent damage to land resources and the ecological environment. It is non-toxic and non-polluting to the environment, and is in line with the low-carbon economy and green environmental protection. In addition, because it can be rapidly degraded into non-toxic and harmless carbon dioxide, inorganic salts and water after use, it does not need to be recycled and processed, and the processing fee is exempted. It has a wide range of applications, low cost, and good environmental and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a picture showing the degradation of the degradable coating film of the present invention in a marine environment within 4 months. DETAILED DESCRIPTION
[0044] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be clearly and completely described below in conjunction with embodiments. The description in this section is only exemplary and explanatory and should not have any limiting effect on the scope of protection of the present invention.
[0045] The invention relates to the following steps: weighing 0.2-3.5 parts of chitosan, 0.2-3.2 parts of organic acid, 0.01-0.4 parts of auxiliary film agent, 0.002-0.05 parts of emulsifier, 0.01-0.05 parts of moisturizer, 0.01-0.03 parts of silicon dioxide and 0.01-0.05 parts of calcium chloride in sequence by weight; placing chitosan and deionized water in a container, stirring the chitosan in the deionized water by magnetic stirring, adding the organic acid thereto, stirring at 300-600 rpm and 30-50° C. for 4-5 hours until the chitosan is completely dissolved, and obtaining a chitosan solution; placing the auxiliary film agent, moisturizer and deionized water in a container, heating the container in a water bath at 30-90° C., and stirring and mixing for 3-4 hours to obtain a mixed solution; and placing the chitosan in a container, stirring the container in a water bath at 30-90° C., and stirring and mixing the mixture for 3-4 hours. The polysaccharide solution is mixed with the mixed solution, and an emulsifier, calcium chloride and silicon dioxide are added to the solution at a temperature of 30-90°C, and stirred for 2-12 hours to obtain a film-forming solution; the film-forming solution is centrifuged at 5000-8000 rpm for 5-15 minutes, and after removing bubbles in the solution, the supernatant is cast on a polytetrafluoroethylene mold, kept at a constant temperature of 30-60°C, dried for 20-48 hours to form a film, and naturally cooled to room temperature; the film is placed in a 25%-40% sodium carbonate solution and soaked for 0.5-5 hours, then horizontally unfolded, and rinsed with deionized water to remove the sodium carbonate remaining on the surface until the pH of the deionized water after washing is 6.5-7.5; the film is dried at a constant temperature of 30-50°C for 0.5-18 hours to form a film, cooled naturally to room temperature, and peeled to obtain a chitosan packaging film.
[0046] Example 1
[0047] According to the weight percentage, 0.5 parts of chitosan, 1 part of acetic acid, 0.1 parts of carrageenan, 0.05 parts of Tween-80, 0.01 parts of glycerol, 0.01 parts of silicon dioxide, and 0.01 parts of calcium chloride were weighed in sequence, with a total weight of 8.35 g; chitosan and deionized water were placed in a container, and chitosan was fully dispersed in 40 parts of deionized water by magnetic stirring, acetic acid was added thereto, and the mixture was stirred at 500 rpm and 35°C for 3 hours until the chitosan was completely dissolved to obtain a chitosan solution; carrageenan, glycerol, and 10 parts of deionized water were placed in a container, heated in a water bath at 30°C, and stirred for 3 hours to obtain a mixed solution; chitosan was added to the container, and the mixture was stirred at 30°C for 3 hours. The sugar solution is mixed with the mixed solution, Tween-80, calcium chloride and silicon dioxide are added to the solution, the temperature is 50°C, and the solution is stirred for 7 hours to obtain a film-forming solution; the film-forming solution is centrifuged at 6000rpm for 7 minutes, and after removing bubbles in the solution, the supernatant is cast on a polytetrafluoroethylene mold, kept at a constant temperature of 55°C, dried for 20 hours to form a film, and naturally cooled to room temperature; the film is placed in a 25% sodium carbonate solution and then horizontally spread out, and rinsed with deionized water to remove the sodium carbonate remaining on the surface until the pH of the deionized water after washing is 7.5; the film is dried at a constant temperature of 30°C for 18 hours to form a film, naturally cooled to room temperature, and peeled off to obtain a chitosan packaging film.
[0048] Example 2
[0049] According to weight, 3 parts of chitosan, 1.5 parts of acetic acid, 0.096 parts of citric acid, 0.2 parts of pectin, 0.05 parts of Tween-80, 0.02 parts of sodium hyaluronate, 0.01 parts of silicon dioxide, and 0.02 parts of calcium chloride were weighed in sequence, with a total weight of 24.48 g; chitosan and deionized water were placed in a container, and chitosan was fully dispersed in 110 parts of deionized water by magnetic stirring, acetic acid and citric acid were added thereto, and the mixture was stirred at 600 rpm and 50°C for 4 hours until the chitosan was completely dissolved to obtain a chitosan solution; pectin, sodium hyaluronate, and 10 parts of deionized water were placed in a container, heated in a water bath at 40°C, and stirred for 4 hours. The method comprises the steps of: obtaining a mixed solution; mixing the chitosan solution with the mixed solution, adding Tween-80, calcium chloride and silicon dioxide to the solution, stirring at a temperature of 55°C for 4 hours to obtain a film-forming solution; centrifuging the film-forming solution at 8000 rpm for 5 minutes, removing bubbles in the solution, casting the supernatant on a polytetrafluoroethylene mold, maintaining a constant temperature of 30°C, drying for 48 hours to form a film, and naturally cooling to room temperature; soaking the film in a 40% sodium carbonate solution for 0.5 hours, unfolding it horizontally, and washing it with deionized water to remove the sodium carbonate remaining on the surface until the pH of the deionized water after washing is 7; drying it at a constant temperature of 35°C for 18 hours to form a film, naturally cooling to room temperature, and peeling it off to obtain a chitosan packaging film.
[0050] Example 3
[0051] According to weight, 1 part of chitosan, 2 parts of acetic acid, 0.014 parts of gelatin, 0.1 parts of Tween-80, 0.01 parts of glycerol, 0.017 parts of silicon dioxide, and 0.02 parts of calcium chloride were weighed in sequence, with a total weight of 15.805 g; chitosan and deionized water were placed in a container, and chitosan was fully dispersed in 40 parts of deionized water by magnetic stirring, acetic acid was added thereto, and the mixture was stirred at 500 rpm and 35°C for 3 hours until the chitosan was completely dissolved to obtain a chitosan solution; gelatin, glycerol, and 10 parts of deionized water were placed in a container, heated in a water bath at 30°C, and stirred for 3 hours to obtain a mixed solution; chitosan was added to the container, and the mixture was stirred at 30°C ... The sugar solution is mixed with the mixed solution, Tween-80, calcium chloride and silicon dioxide are added to the solution, the temperature is 50°C, and the solution is stirred for 7 hours to obtain a film-forming solution; the film-forming solution is centrifuged at 6000rpm for 7 minutes, and after removing bubbles in the solution, the supernatant is cast on a polytetrafluoroethylene mold, kept at a constant temperature of 50°C, dried for 24 hours to form a film, and naturally cooled to room temperature; the film is placed in a 25% sodium carbonate solution and then horizontally spread out, and rinsed with deionized water to remove the sodium carbonate remaining on the surface until the pH of the deionized water after washing is 7.5; the film is dried at a constant temperature of 30°C for 18 hours to form a film, naturally cooled to room temperature, and peeled off to obtain a chitosan packaging film.
[0052] Example 4
[0053] According to the weight percentage, 1.8 parts of chitosan, 0.9 parts of acetic acid, 0.0072 parts of tartaric acid, 0.12 parts of pectin, 0.003 parts of polyvinyl pyrrolidone, 0.01 parts of glycerol, 0.01 parts of silicon dioxide, and 0.02 parts of calcium chloride were weighed in sequence, with a total weight of 14.351 g; chitosan and 85 parts of deionized water were placed in a container, and the chitosan was fully dispersed in the deionized water by magnetic stirring, acetic acid and tartaric acid were added thereto, and the mixture was stirred at 600 rpm and 30°C for 5 hours until the chitosan was completely dissolved to obtain a chitosan solution; pectin, polyvinyl pyrrolidone, and 10 parts of deionized water were placed in a container, heated in a water bath at 30°C, and stirred for 4 hours , obtaining a mixed solution; mixing the chitosan solution with the mixed solution, adding polyvinyl pyrrolidone, calcium chloride and silicon dioxide to the solution, stirring at a temperature of 60°C for 4 hours to obtain a film-forming solution; centrifuging the film-forming solution at 5000rpm for 15 minutes, removing bubbles in the solution, casting the supernatant on a polytetrafluoroethylene mold, keeping a constant temperature of 60°C, drying for 20 hours to form a film, and naturally cooling to room temperature; soaking the film in a 30% sodium carbonate solution for 2 hours, then spreading it horizontally, rinsing it with deionized water to remove the residual sodium carbonate on the surface, until the pH of the deionized water after washing is 7.5; drying it at a constant temperature of 50°C for 0.5 hours to form a film, naturally cooling to room temperature, and peeling it off to obtain a chitosan packaging film.
[0054] Example 5
[0055] According to the weight percentage, 2 parts of chitosan, 1 part of acetic acid, 0.096 parts of citric acid, 0.2 parts of xanthan gum, 0.02 parts of Tween-80, 0.05 parts of glycerol, 0.03 parts of silicon dioxide, and 0.05 parts of calcium chloride were weighed in sequence, with a total weight of 17.23 g; chitosan and deionized water were placed in a container, and chitosan was fully dispersed in 100 parts of deionized water by magnetic stirring, acetic acid and citric acid were added thereto, and the mixture was stirred at 600 rpm and 30°C for 5 hours until the chitosan was completely dissolved to obtain a chitosan solution; xanthan gum, glycerol, and 10 parts of deionized water were placed in a container, heated in a water bath at 50°C, and stirred for 3 hours to obtain The method comprises the following steps: mixing the chitosan solution with the mixed solution, adding Tween-80, calcium chloride and silicon dioxide to the solution, stirring for 5 hours at a temperature of 30°C to obtain a film-forming solution; centrifuging the film-forming solution at 8000 rpm for 5 minutes, removing bubbles in the solution, casting the supernatant on a polytetrafluoroethylene mold, drying at a constant temperature of 45°C for 25 hours to form a film, and naturally cooling to room temperature; soaking the film in a 35% sodium carbonate solution for 3 hours, unfolding it horizontally, and rinsing it with deionized water to remove the residual sodium carbonate on the surface until the pH of the deionized water after washing is 6.5; drying at a constant temperature of 50°C for 1 hour to form a film, naturally cooling to room temperature, and peeling it off to obtain a chitosan packaging film.
[0056] Example 6
[0057] According to the weight percentage, 3 parts of chitosan, 1.5 parts of acetic acid, 0.096 parts of citric acid, 0.3 parts of potato starch, 0.05 parts of Tween-80, 0.02 parts of sodium hyaluronate, 0.01 parts of silicon dioxide, and 0.02 parts of calcium chloride were weighed in sequence, with a total weight of 24.98 g; chitosan and deionized water were placed in a container, and chitosan was fully dispersed in 110 parts of deionized water by magnetic stirring, acetic acid and citric acid were added thereto, and the mixture was stirred at 600 rpm and 50°C for 4 hours until the chitosan was completely dissolved to obtain a chitosan solution; potato starch, sodium hyaluronate, and 10 parts of deionized water were placed in a container, heated in a water bath at 90°C, and stirred to mix. 4h to obtain a mixed solution; the chitosan solution was mixed with the mixed solution, Tween-80, calcium chloride and silicon dioxide were added to the solution at 55°C, and stirred for 4h to obtain a film-forming solution; the film-forming solution was centrifuged at 8000rpm for 5min, and after removing the bubbles in the solution, the supernatant was cast on a polytetrafluoroethylene mold, kept at a constant temperature of 30°C, dried for 48h to form a film, and naturally cooled to room temperature; the film was placed in a 40% sodium carbonate solution and soaked for 0.5h, then spread horizontally, and rinsed with deionized water to remove the residual sodium carbonate on the surface until the pH of the deionized water after washing was 7; dried at a constant temperature of 35°C for 18h to form a film, cooled naturally to room temperature, and peeled off to obtain a chitosan packaging film.
[0058] Comparative Example
[0059] According to the weight percentage, 2 parts of chitosan, 1 part of acetic acid, 97 parts of deionized water, 0.05 parts of glycerol, and 0.02 parts of sodium hyaluronate are weighed in sequence. Chitosan powder and deionized water are placed in a container, and chitosan is fully dispersed in deionized water by magnetic stirring at 300-600rpm, acetic acid is added thereto, and the mixture is stirred at a speed of 700rpm and a temperature of 30°C for 4h until chitosan is completely dissolved to obtain a chitosan solution; the chitosan solution is mixed with glycerol, and stirred at a speed of 700rpm and a temperature of 40°C for 8h to obtain a film-forming liquid; the above-mentioned film-forming liquid is ultrasonically treated at an ultrasonic frequency of 70kHz, and then placed in a vacuum degassing machine for 40min, cast on a horizontal polytetrafluoroethylene mold, and dried in an oven at a constant temperature of 50°C for 24h to form a film; it is naturally cooled to room temperature, peeled off, and a traditional chitosan film is obtained.
[0060] The mechanical properties of the film products obtained in Examples 1-6 and Comparative Examples were tested according to GB / T1040.3-2006. The films were cut into 10 mm × 100 mm rectangles and tested for tensile strength and elongation at break using a universal material testing machine at a test speed of 100 mm / min and an initial clamping distance of 50 mm. The test was repeated 3 times for each group of films.
[0061] The swelling performance test method of the film products obtained in Examples 1-6 and Comparative Examples is as follows: the film was cut into 1×1 cm size, dried at 70°C for 12 hours, and then soaked in 25 mL of deionized water for 2 hours. The film was taken out of the water with tweezers and the surface adsorbed water was removed with absorbent paper for 30 seconds, and then the weight of the film was weighed and recorded. The swelling performance of the chitosan film was calculated according to formula (1):
[0062] Swelling rate (%) = (W2-W1) / W1×100% (1)
[0063] Where: W1 is the initial mass of the film; W2 is the final mass of the film after swelling; each group of samples was measured three times and the average value was calculated.
[0064] The results are shown in Table 1:
[0065] Table 1 Parameters characterizing product performance
[0066]
[0067] It can be seen from the test results in Table 1 that the tensile strength and elongation at break of the chitosan packaging film provided by the present invention are significantly improved compared with traditional chitosan films.
[0068] According to GB / T 40611-2021, the biodegradable film of the present invention is easily eroded and broken by seawater in the marine environment, can enrich the bacterial colony, and is basically degraded in 4 months without obvious film residue (see Figure 1 ), has excellent degradability.
Claims
1. A method for preparing a high-strength degradable chitosan packaging film, characterized in that: The composition is as follows according to the weight ratio: 0.2-3.5 parts of chitosan, 0.2-3.2 parts of organic acid, 0.01-0.4 parts of auxiliary film agent, 0.002-0.05 parts of emulsifier, 0.01-0.05 parts of moisturizer, 0.01-0.03 parts of silicon dioxide, 0.01-0.05 parts of calcium chloride; The preparation steps of the chitosan packaging film are: Step 1: Weigh each raw material in order according to its composition; Step 2: placing chitosan and deionized water in a container, stirring to fully disperse the chitosan in the deionized water, adding an organic acid to the container, heating and stirring until the chitosan is completely dissolved, to obtain a chitosan solution; Step 3: placing the auxiliary film agent, moisturizing agent and deionized water in a container, heating and stirring to mix, and obtaining a mixed solution; Step 4: mixing the chitosan solution with the mixed solution, heating and stirring; Step 5: Add emulsifier, calcium chloride and silicon dioxide to the above solution, and continue stirring to obtain a film-forming solution; Step 6: Centrifuge the film-forming solution, remove bubbles from the solution, cast it on a mold, dry it at a constant temperature to form a film, and cool it naturally to room temperature; Step 7: Soak the film in a sodium carbonate solution for 0.5-5 hours; Step 8: Spread the film horizontally and rinse it with deionized water to remove the residual sodium carbonate on the surface until the pH of the deionized water after washing is 6.5-7.5; Step 9: After constant temperature drying to form a film, it is naturally cooled to room temperature and peeled off to obtain a chitosan packaging film.
2. The method for preparing a high-strength degradable chitosan packaging film according to claim 1, characterized in that: The chitosan is the main material of the membrane, which is degradable and does not cause environmental pollution. Its sources include: the shells of marine arthropods such as shrimps and crabs.
3. The method for preparing the high-strength degradable chitosan packaging film according to claim 1, characterized in that: The organic acid is one or more of acetic acid, lactic acid, ascorbic acid, citric acid, malic acid, succinic acid, adipic acid and tartaric acid; the auxiliary film agent is one or more of pectin, carrageenan, gelatin, agar, starch, xanthan gum, guardo gum and sodium alginate.
4. The method for preparing a high-strength degradable chitosan packaging film according to claim 1, characterized in that: The emulsifier is one or more of sucrose stearate, Tween 80, and polyvinyl pyrrolidone; The moisturizing agent is one or more of glycerol, 1,3-butylene glycol, 1,3-propylene glycol, polyethylene glycol, sodium carboxymethyl cellulose, sodium hyaluronate, polypropylene glycol and sorbitol.
5. The method for preparing the high-strength degradable chitosan packaging film according to claim 1, characterized in that: In step 2, the mass ratio of chitosan to water in the chitosan aqueous solution is 1:95-1:
36.
6. The method for preparing the high-strength degradable chitosan packaging film according to claim 1, characterized in that: In step 2, the heating and stirring reaction conditions are a temperature of 30-50° C. and a time of 3-4 h; In step 3, the heating and stirring reaction conditions are a temperature of 30-90° C. and a time of 3-4 hours; in step 3, the mass ratio of the auxiliary membrane agent to deionized water is 1:3000-1:400, and the mass ratio of the moisturizer to the auxiliary membrane agent is 1:15-5:
7.
7. The method for preparing the high-strength degradable chitosan packaging film according to claim 1, characterized in that: In step 4, the heating and stirring reaction conditions are a temperature of 30-90° C. and a time of 2-12 h.
8. The method for preparing the high-strength degradable chitosan packaging film according to claim 1, characterized in that: In step 6, the centrifugal speed is 5000-8000 rpm, and the centrifugal time is 5-15 min; The constant temperature drying conditions are 30-60° C. and 20-48 hours. The mold is a horizontal polytetrafluoroethylene mold.
9. The method for preparing the high-strength degradable chitosan packaging film according to claim 1, characterized in that: In step 7, the concentration range of the sodium carbonate solution is 25%-40%; In step 9, the constant temperature drying conditions are a temperature of 30-50° C. and a time of 0.5-18 h.
10. A high-strength degradable chitosan packaging film prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The chitosan packaging film has a tensile strength of 27.61 to 41.12 MPa and an elongation at break of 4.33 to 5.34%; The chitosan packaging film is easily eroded and broken by seawater in a marine environment, can enrich bacterial colonies, and degrades in 4 months without obvious film residue.
Citation Information
Patent Citations
Edible biological preservative film and preparation method thereof
CN104194354A
Chitosan biomembrane
CN105384974A
Edible composite film, and preparing method and application thereof
CN108639564A
Food preservative film and preparation method thereof
CN108912358A
Method for preparing protein / pectin / chitosan composite film by using thermostable recombinant bacterial laccase, and product thereof, and applications of product
CN109111584A