Antistatic polyether-ether-ketone composite material and preparation method thereof

By adding carbon nanotube composite conductive agent, modified graphene and carbon fiber to polyether ether ketone, the problem of insufficient electrostatic properties of polyether ether ketone materials is solved, and the conductive and mechanical properties are improved, making it suitable for applications in electrostatic environments. .

CN118772573AInactive Publication Date: 2024-10-15ZHEJIANG BROTHER NEW MATERIAL CO LTD

Patent Information

Application Number
CN202410852270.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional polyetheretherketone materials have poor electrostatic performance and are prone to accumulation of electrostatic charges and cause electrostatic discharge problems, making it difficult to meet the requirements for electrostatic properties of materials in specific application fields.

Method used

Carbon nanotube composite conductive agent, modified graphene and carbon fiber are used as conductive fillers. Melt blending and granulation are carried out through a mixer and twin-screw extruder to prepare antistatic polyetheretherketone composite materials to improve its conductive properties and mechanics. performance.

Benefits of technology

It significantly improves the electrical conductivity of composite materials, reduces the risk of static electricity accumulation and discharge, enhances mechanical properties, and maintains stable performance in high-temperature environments. It is suitable for automotive, electronics, aviation and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772573A_ABST
    Figure CN118772573A_ABST
Patent Text Reader

Abstract

The invention relates to the field of engineering plastic compounding, in particular to an antistatic polyether-ether-ketone composite material which is prepared from the following raw materials in parts by weight: 85-100 parts of polyether-ether-ketone, 1-5 parts of a carbon nanotube composite conductive agent, 1-5 parts of carbon fibers and 1-5 parts of modified graphene. According to the invention, by optimizing the raw material ratio and processing conditions, the thermoplastic polyether-ether-ketone is taken as a matrix, the carbon nanotube composite conductive agent, the modified graphene and the chopped carbon fiber are taken as conductive fillers, and the polyether-ether-ketone composite material with good antistatic property is obtained by melt blending and extrusion under the condition of ensuring the excellent performance of the polyether-ether-ketone. The antistatic polyether-ether-ketone composite material is suitable for the fields of automobiles, electronics, aviation and the like, and the antistatic polyether-ether-ketone composite material adopting the carbon nanotubes, the graphene and the carbon fibers as the conductive filler has the beneficial effects of improving the conductivity, enhancing the mechanical property, reducing the weight, improving the heat resistance and the like, and is suitable for the application fields needing antistatic performance and excellent performance at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of engineering plastic composites, and in particular to an antistatic polyetheretherketone composite material and a preparation method thereof. Background Art

[0002] Polyetheretherketone, English name poly (ether-ether-ketone), referred to as PEEK, contains a rigid benzene ring in its molecular structure, so it has excellent high temperature resistance, mechanical properties, electrical insulation, chemical resistance and other characteristics. At the same time, its molecular structure contains ether bonds, which makes it flexible, so it can be processed by thermoplastic engineering plastics molding method.

[0003] In the fields of aerospace, electronics, automobiles, etc., high-performance materials with antistatic properties are needed. Traditional polyetheretherketone materials usually have excellent mechanical properties and high temperature resistance, but perform poorly in terms of static electricity, easily accumulate static charges and cause electrostatic discharge problems. Therefore, researchers have begun to focus on the development of polyetheretherketone composite materials with antistatic properties to meet the requirements of material electrostatic properties in specific application fields.

[0004] In summary, the development of an antistatic polyetheretherketone composite material and a preparation method thereof is still a key issue that needs to be urgently addressed in the field of engineering plastic composites. Summary of the invention

[0005] In view of the problems existing in the prior art, the object of the present invention is to provide an antistatic polyetheretherketone composite material and a preparation method thereof.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] An antistatic polyetheretherketone composite material is composed of the following raw materials and their weight proportions: 85-100 parts of polyetheretherketone, 1-5 parts of carbon nanotube composite conductive agent, 1-5 parts of carbon fiber and 1-5 parts of modified graphene.

[0008] The present invention is further configured as follows: the melt flow rate of the polyetheretherketone is 5 to 100 g / 10 min.

[0009] The present invention is further configured as follows: the short cut length of the carbon fiber is 2 to 5 mm, the diameter is 7 to 8 μm, and the bulk density is 0.53 to 0.56 g / cm 3 .

[0010] The present invention is further configured as follows: the raw materials of the carbon nanotube composite conductive agent include an amino acid aqueous solution, carbon nanotubes and a conductive filler, the mass fraction of the amino acid in the amino acid aqueous solution is 0.1% to 8%, and the amino acid in the amino acid aqueous solution can form a π-π effect with the carbon nanotubes, and the mass ratio of the amino acid, carbon nanotubes and conductive filler is 0.1 to 10:1 to 35:0 to 15.

[0011] The present invention is further configured as follows: the amino acid is selected from at least one of lysine, phenylalanine and tryptophan, the carbon nanotube is selected from at least one of single-walled carbon nanotube and multi-walled carbon nanotube, and the conductive filler is selected from at least one of carbon black and graphite.

[0012] The present invention is further configured as follows: the raw materials of the modified graphene include graphene, a polymer surfactant, an inorganic salt and carbon black, the graphene is selected from at least one of graphene oxide, thin-layer graphene and multi-layer graphene, the polymer surfactant is selected from at least one of dodecyl polyoxyethylene ether and octanol polyoxyethylene ether, the inorganic salt is selected from at least one of ammonium borate, ammonium nitrate and ammonium carbonate, and the carbon black is selected from at least one of acetylene black, Ketjen black and superconducting carbon black.

[0013] A method for preparing an antistatic polyetheretherketone composite material comprises the following steps:

[0014] Ⅰ. Preparation of carbon nanotube composite conductive agent;

[0015] II. Preparation of modified graphene;

[0016] III. Accurately weigh each raw material according to its weight ratio;

[0017] IV. Mixing with a mixer: using a mixer to mix the polyetheretherketone, the carbon nanotube composite conductive agent and the modified graphene according to the above proportions, and mixing them evenly to obtain a mixed material;

[0018] V. Use a twin-screw extruder for extrusion granulation. The temperature of each zone of the extruder is set to 320±40°C, the head temperature is 360±20°C, and the speed of the twin-screw extruder is 200-500rpm. After the temperature of each zone of the extruder is stable, the mixed material is fed into the twin-screw extruder from the main feeding port, and the carbon fiber is fed into the twin-screw extruder from the side feeding port;

[0019] VI. Extrusion granulation: A twin-screw extruder is used to melt-mix the mixed material and the carbon fiber and extrude the mixed material into granules, and the extruded sample is air-cooled to room temperature and then pelletized to obtain a polyetheretherketone composite material.

[0020] The present invention is further configured as follows: in step I, the following steps are included:

[0021] A1. Pretreatment: Pretreat carbon nanotubes and conductive fillers to remove impurities and impurities to ensure that the subsequent modification reaction can proceed smoothly;

[0022] A2. Introduction of amino acids: Select a suitable amino acid as a modifier, dissolve it in a solvent to obtain an amino acid aqueous solution, mix the amino acid aqueous solution, carbon nanotubes and conductive filler according to a mass ratio, and stir and disperse them uniformly;

[0023] A3. Post-reaction treatment: After the reaction is completed, the product is washed, centrifuged and dried to remove unreacted amino acids and solvent residues to obtain a carbon nanotube composite conductive agent.

[0024] The present invention is further configured as follows: in step II, the following steps are included:

[0025] B1. dissolving a polymer surfactant in a solvent to obtain an aqueous solution of the polymer surfactant, wherein the concentration of the aqueous solution of the polymer surfactant is 3 to 10 mg / ml;

[0026] B2, adding graphene powder to a polymer surfactant aqueous solution and performing ultrasonic stripping at a rotation speed of 3000-4000 r / min, centrifuging for 20-40 min to obtain a graphene suspension, then filtering and washing with water to a pH of 7 to obtain pretreated graphene;

[0027] B3, mixing the pretreated graphene and the inorganic salt in a mass ratio of 1-4:2-8 and grinding for 30 minutes, and then subjecting the mixture to microwave exfoliation for 5-10 minutes at a power of 500-1000 W to obtain layered graphene;

[0028] B4. Mix the layered graphene and carbon black in a mass ratio of 5-15:1-5, and thermally decompose them in a muffle furnace under a nitrogen atmosphere for 60 minutes at a temperature of 900-1000° C. to obtain modified graphene.

[0029] Beneficial Effects

[0030] Compared with the known public technology, the technical solution provided by the present invention has the following advantages:

[0031] Beneficial effects:

[0032] (1) In the present invention, carbon nanotubes, graphene and carbon fibers have excellent electrical conductivity. Adding them as conductive fillers into the polyetheretherketone matrix can significantly improve the electrical conductivity of the composite material and effectively reduce the resistance of the material, thereby reducing the risk of static electricity accumulation and discharge.

[0033] (2) In the present invention, carbon nanotubes and carbon fibers generally have the characteristics of high strength and high modulus. Introducing them into the polyetheretherketone matrix can enhance the mechanical properties of the composite material, improve its tensile strength, bending resistance and other properties, and make the material more durable.

[0034] (3) In the present invention, carbon nanotubes and carbon fibers have the characteristic of being lightweight. When added to the polyetheretherketone matrix, the density of the composite material can be reduced, thereby reducing the overall weight. The composite material is therefore suitable for use in applications that have high requirements on material weight.

[0035] (4) In the present invention, carbon nanotubes, graphene and carbon fibers have good high temperature resistance. Using them as conductive fillers can improve the heat resistance of composite materials, so that the materials can still maintain stable performance in high temperature environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The present invention is a flow chart of an antistatic polyetheretherketone composite material and a preparation method thereof. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The present invention will be further described below in conjunction with the embodiments.

[0039] Example 1

[0040] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material, which is composed of the following raw materials and their weight parts: 96 parts of polyetheretherketone, 1 part of carbon nanotube composite conductive agent, 2 parts of carbon fiber, and 1 part of modified graphene;

[0041] Among them, the melt flow rate of polyetheretherketone is 5g / 10min, the short length of carbon fiber is 2mm, the diameter is 7μm, and the bulk density is 0.53g / cm 3 , the short-cut carbon fiber has improved bonding with the resin after special sizing, increased the packing density, and is easy to process;

[0042] Furthermore, the raw materials of the carbon nanotube composite conductive agent include an amino acid aqueous solution, carbon nanotubes and a conductive filler, the mass fraction of the amino acid in the amino acid aqueous solution is 0.1%, and the amino acid in the amino acid aqueous solution can form a π-π interaction with the carbon nanotubes, and the mass ratio of the amino acid, the carbon nanotubes and the conductive filler is 0.1:1:3;

[0043] The amino acid is lysine, the carbon nanotube is single-walled carbon nanotube, and the conductive filler is carbon black.

[0044] Furthermore, the raw materials of the modified graphene include graphene, polymer surfactant, inorganic salt and carbon black, the graphene is graphene oxide, the polymer surfactant is dodecyl polyoxyethylene ether, the inorganic salt is ammonium borate, and the carbon black is acetylene black;

[0045] A method for preparing an antistatic polyetheretherketone composite material comprises the following steps:

[0046] Ⅰ. Preparation of carbon nanotube composite conductive agent, including the following steps:

[0047] A1. Pretreatment: Pretreat carbon nanotubes and conductive fillers to remove impurities and impurities to ensure that the subsequent modification reaction can proceed smoothly;

[0048] A2. Introduction of amino acids: Select a suitable amino acid as a modifier, dissolve it in a solvent to obtain an amino acid aqueous solution, mix the amino acid aqueous solution, carbon nanotubes and conductive filler according to a mass ratio, and stir and disperse them uniformly;

[0049] A3. Post-reaction treatment: After the reaction is completed, the product is washed, centrifuged and dried to remove unreacted amino acids and solvent residues to obtain a carbon nanotube composite conductive agent;

[0050] II. Preparation of modified graphene, comprising the following steps:

[0051] B1, dissolving a polymer surfactant in a solvent to obtain an aqueous solution of the polymer surfactant, wherein the concentration of the aqueous solution of the polymer surfactant is 3 mg / ml;

[0052] B2, adding graphene powder to a polymer surfactant aqueous solution and performing ultrasonic stripping at a rotation speed of 3000r / min, centrifuging for 20min to obtain a graphene suspension, then filtering and washing with water to a pH of 7 to obtain pretreated graphene;

[0053] B3, the pretreated graphene and the inorganic salt were mixed and ground at a mass ratio of 1:2 for 30 minutes, and then microwave exfoliation was performed for 5 minutes at a power of 500 W to obtain layered graphene;

[0054] B4, mixing the layered graphene and carbon black in a mass ratio of 5:1, and thermally decomposing them in a muffle furnace under a nitrogen atmosphere for 60 min at a temperature of 900° C. to obtain modified graphene;

[0055] III. Accurately weigh each raw material according to its weight ratio;

[0056] IV. Mixing with a mixer: using a mixer to mix the polyetheretherketone, the carbon nanotube composite conductive agent and the modified graphene according to the above proportions, and mixing them evenly to obtain a mixed material;

[0057] V. Use a twin-screw extruder for extrusion granulation, the temperatures of each zone of the extruder are set to 280°C, 330°C, 350°C, 350°C, 340°C, 340°C, 340°C, 340°C, 350°C, 350°C, 340°C, 340°C, 340°C, 340°C, the head temperature is 360°C, the main screw speed of the twin-screw extruder is 500rpm, and the side screw speed is 200-400rpm. After the temperatures of each zone of the extruder are stable, the mixed material is fed into the twin-screw extruder from the main feeding port, and the carbon fiber is fed into the twin-screw extruder from the side feeding port;

[0058] VI. Extrusion granulation: A twin-screw extruder is used to melt-mix the mixed material and carbon fiber for extrusion granulation, and the extruded sample is air-cooled to room temperature and then pelletized. The pellets cut out are cylindrical granular materials, and a polyetheretherketone composite material is obtained.

[0059] Example 2

[0060] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material, which is composed of the following raw materials and their weight parts: 96 parts of polyetheretherketone, 3 parts of carbon fiber, and 1 part of modified graphene;

[0061] Among them, the melt flow rate of polyetheretherketone is 50g / 10min, the short length of carbon fiber is 3mm, the diameter is 7μm, and the bulk density is 0.55g / cm 3 , the short-cut carbon fiber has improved bonding with the resin after special sizing, increased the packing density, and is easy to process;

[0062] Furthermore, the raw materials of the modified graphene include graphene, polymer surfactant, inorganic salt and carbon black, the graphene is thin-layer graphene, the polymer surfactant is octanol polyoxyethylene ether, the inorganic salt is ammonium nitrate and ammonium carbonate, and the carbon black is Ketjen black and superconducting carbon black;

[0063] A method for preparing an antistatic polyetheretherketone composite material comprises the following steps:

[0064] Ⅰ. Preparation of modified graphene, comprising the following steps:

[0065] B1, dissolving a polymer surfactant in a solvent to obtain an aqueous solution of the polymer surfactant, wherein the concentration of the aqueous solution of the polymer surfactant is 5 mg / ml;

[0066] B2, adding graphene powder to a polymer surfactant aqueous solution and performing ultrasonic stripping at a rotation speed of 3500r / min, centrifuging for 30min to obtain a graphene suspension, then filtering and washing with water to a pH of 7 to obtain pretreated graphene;

[0067] B3, the pretreated graphene and the inorganic salt were mixed and ground at a mass ratio of 2:5 for 30 minutes, and then microwave exfoliation was performed for 8 minutes at a power of 800 W to obtain layered graphene;

[0068] B4, mixing the layered graphene and carbon black in a mass ratio of 5:2, and thermally decomposing them in a muffle furnace under a nitrogen atmosphere for 60 min at a temperature of 950° C. to obtain modified graphene;

[0069] Ⅱ. Accurately weigh each raw material according to its weight ratio;

[0070] III. Mixing with a mixer: using a mixer to mix the polyetheretherketone and the modified graphene according to the above ratio, so as to mix them evenly to obtain a mixed material;

[0071] IV. Use a twin-screw extruder for extrusion granulation. The temperatures in each zone of the extruder are set to 280°C, 330°C, 350°C, 350°C, 340°C, 340°C, 340°C, 340°C, 350°C, 350°C, 340°C, 340°C, 340°C, 340°C, and the head temperature is 360°C. The main screw speed of the twin-screw extruder is 500rpm, and the side screw speed is 200-400rpm. After the temperatures in each zone of the extruder are stable, the mixed material is fed into the twin-screw extruder from the main feeding port, and the carbon fiber is fed into the twin-screw extruder from the side feeding port.

[0072] V. Extrusion granulation: A twin-screw extruder is used to melt-mix the mixed material and carbon fiber for extrusion granulation, and the extruded sample is air-cooled to room temperature and then pelletized. The pellets cut out are cylindrical granular materials, and a polyetheretherketone composite material is obtained.

[0073] Example 3

[0074] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material, which is composed of the following raw materials and their weight parts: 96 parts of polyetheretherketone, 1 part of carbon nanotube composite conductive agent, and 3 parts of carbon fiber;

[0075] Among them, the melt flow rate of polyetheretherketone is 80g / 10min, the short length of carbon fiber is 5mm, the diameter is 8μm, and the bulk density is 0.56g / cm 3 , the short-cut carbon fiber has improved bonding with the resin after special sizing, increased the packing density, and is easy to process;

[0076] Furthermore, the raw materials of the carbon nanotube composite conductive agent include an amino acid aqueous solution, carbon nanotubes and a conductive filler, the mass fraction of the amino acid in the amino acid aqueous solution is 0.7%, and the amino acid in the amino acid aqueous solution can form a π-π interaction with the carbon nanotubes, and the mass ratio of the amino acid, the carbon nanotubes and the conductive filler is 3:7:2;

[0077] The amino acids are lysine and tryptophan, the carbon nanotubes are single-walled carbon nanotubes, and the conductive filler is carbon black.

[0078] A method for preparing an antistatic polyetheretherketone composite material comprises the following steps:

[0079] Ⅰ. Preparation of carbon nanotube composite conductive agent, including the following steps:

[0080] A1. Pretreatment: Pretreat carbon nanotubes and conductive fillers to remove impurities and impurities to ensure that the subsequent modification reaction can proceed smoothly;

[0081] A2. Introduction of amino acids: Select a suitable amino acid as a modifier, dissolve it in a solvent to obtain an amino acid aqueous solution, mix the amino acid aqueous solution, carbon nanotubes and conductive filler according to a mass ratio, and stir and disperse them uniformly;

[0082] A3. Post-reaction treatment: After the reaction is completed, the product is washed, centrifuged and dried to remove unreacted amino acids and solvent residues to obtain a carbon nanotube composite conductive agent;

[0083] Ⅱ. Accurately weigh each raw material according to its weight ratio;

[0084] III. Mixing with a mixer: using a mixer to mix the polyetheretherketone and the carbon nanotube composite conductive agent according to the above ratio, so as to mix them evenly to obtain a mixed material;

[0085] IV. Use a twin-screw extruder for extrusion granulation. The temperatures in each zone of the extruder are set to 280°C, 330°C, 350°C, 350°C, 340°C, 340°C, 340°C, 340°C, 350°C, 350°C, 340°C, 340°C, 340°C, 340°C, and the head temperature is 360°C. The main screw speed of the twin-screw extruder is 500rpm, and the side screw speed is 200-400rpm. After the temperatures in each zone of the extruder are stable, the mixed material is fed into the twin-screw extruder from the main feeding port, and the carbon fiber is fed into the twin-screw extruder from the side feeding port.

[0086] V. Extrusion granulation: A twin-screw extruder is used to melt-mix the mixed material and carbon fiber for extrusion granulation, and the extruded sample is air-cooled to room temperature and then pelletized. The pellets cut out are cylindrical granular materials, and a polyetheretherketone composite material is obtained.

[0087] Example 4

[0088] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material, which is composed of the following raw materials and their weight parts: 96 parts of polyetheretherketone, 1 part of carbon nanotube composite conductive agent, and 3 parts of modified graphene;

[0089] Among them, the melt flow rate of polyetheretherketone is 100g / 10min;

[0090] Furthermore, the raw materials of the carbon nanotube composite conductive agent include an amino acid aqueous solution, carbon nanotubes and a conductive filler, the mass fraction of the amino acid in the amino acid aqueous solution is 8%, and the amino acid in the amino acid aqueous solution can form a π-π interaction with the carbon nanotubes, and the mass ratio of the amino acid, the carbon nanotubes and the conductive filler is 10:35:14;

[0091] Among them, the amino acids are phenylalanine and tryptophan, the carbon nanotubes are single-walled carbon nanotubes, and the conductive filler is carbon black;

[0092] Furthermore, the raw materials of the modified graphene include graphene, polymer surfactant, inorganic salt and carbon black, the graphene is selected from thin-layer graphene and multi-layer graphene, the polymer surfactant is selected from dodecyl polyoxyethylene ether, the inorganic salt is selected from ammonium borate, and the carbon black is selected from acetylene black, Ketjen black and superconducting carbon black;

[0093] A method for preparing an antistatic polyetheretherketone composite material comprises the following steps:

[0094] Ⅰ. Preparation of carbon nanotube composite conductive agent, including the following steps:

[0095] A1. Pretreatment: Pretreat carbon nanotubes and conductive fillers to remove impurities and impurities to ensure that the subsequent modification reaction can proceed smoothly;

[0096] A2. Introduction of amino acids: Select a suitable amino acid as a modifier, dissolve it in a solvent to obtain an amino acid aqueous solution, mix the amino acid aqueous solution, carbon nanotubes and conductive filler according to a mass ratio, and stir and disperse them uniformly;

[0097] A3. Post-reaction treatment: After the reaction is completed, the product is washed, centrifuged and dried to remove unreacted amino acids and solvent residues to obtain a carbon nanotube composite conductive agent;

[0098] II. Preparation of modified graphene, comprising the following steps:

[0099] B1, dissolving a polymer surfactant in a solvent to obtain an aqueous solution of the polymer surfactant, wherein the concentration of the aqueous solution of the polymer surfactant is 10 mg / ml;

[0100] B2, adding graphene powder to a polymer surfactant aqueous solution and performing ultrasonic stripping at a rotation speed of 4000r / min, centrifuging for 40min to obtain a graphene suspension, then filtering and washing with water to a pH of 7 to obtain pretreated graphene;

[0101] B3, the pretreated graphene and the inorganic salt were mixed and ground at a mass ratio of 1:2 for 30 minutes, and then microwave exfoliation was performed for 10 minutes at a power of 1000 W to obtain layered graphene;

[0102] B4, mixing the layered graphene and carbon black in a mass ratio of 3:1, and thermally decomposing them in a muffle furnace under a nitrogen atmosphere for 60 min at a temperature of 1000° C. to obtain modified graphene;

[0103] III. Accurately weigh each raw material according to its weight ratio;

[0104] IV. Mixing with a mixer: using a mixer to mix the polyetheretherketone, the carbon nanotube composite conductive agent and the modified graphene according to the above proportions, and mixing them evenly to obtain a mixed material;

[0105] V. Use a twin-screw extruder for extrusion granulation, the temperatures of each zone of the extruder are set to 280°C, 330°C, 350°C, 350°C, 340°C, 340°C, 340°C, 340°C, 350°C, 350°C, 340°C, 340°C, 340°C, 340°C, the head temperature is 360°C, the main screw speed of the twin-screw extruder is 500rpm, and the side screw speed is 200-400rpm. After the temperatures of each zone of the extruder are stable, the mixed material is fed into the twin-screw extruder from the main feeding port;

[0106] VI. Extrusion granulation: A twin-screw extruder is used to melt-mix the mixed material and extrude it into granules, and the extruded sample is air-cooled to room temperature and then pelletized. The pellets cut out are cylindrical granular materials, and a polyetheretherketone composite material is obtained.

[0107] Comparative Example 1

[0108] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material and a preparation method thereof, and the preparation method thereof is substantially the same as that of embodiment 1, the main difference being: 2 parts of carbon nanotubes and 2 parts of carbon fibers.

[0109] Comparative Example 2

[0110] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material and a preparation method thereof, and the preparation method is roughly the same as that of Example 1, with the main difference being: 2 parts of carbon fiber and 2 parts of graphene.

[0111] Comparative Example 3

[0112] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material and a preparation method thereof, and the preparation method is roughly the same as that of Example 1, with the main difference being: 1 part of carbon nanotubes, 1 part of graphene, and 2 parts of carbon fibers.

[0113] Comparative Example 4

[0114] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material and a preparation method thereof, and the preparation method is roughly the same as that of Example 1, with the main difference being: 1 part of carbon nanotube composite conductive agent, 1 part of graphene, and 2 parts of carbon fiber.

[0115] Comparative Example 5

[0116] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material and a preparation method thereof, and the preparation method is roughly the same as that of Example 1, the main difference being: 1 part of carbon nanotube composite conductive agent, 1 part of carbon nanotubes, and 2 parts of carbon fiber.

[0117] Comparative Example 6

[0118] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material and a preparation method thereof, and the preparation method is roughly the same as that of Example 1, the main difference being: 1 part of modified graphene, 1 part of graphene, and 2 parts of carbon fiber.

[0119] Comparative Example 7

[0120] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material and a preparation method thereof, and the preparation method is roughly the same as that of Example 1, with the main difference being: 1 part of carbon nanotubes, 1 part of modified graphene, and 2 parts of carbon fibers.

[0121] Comparative Example 8

[0122] Please refer to Figure 1 As shown, this embodiment provides an antistatic polyetheretherketone composite material and a preparation method thereof, and the preparation method thereof is substantially the same as that of embodiment 1, the main difference being that no conductive filler is added.

[0123] Test Trial:

[0124] The polyetheretherketone composite materials prepared by Examples 1 to 4 are recorded as Example Groups 1 to 4, and the polyetheretherketone composite materials prepared by Comparative Examples 1 to 8 are recorded as Comparative Groups 1 to 8. The polyetheretherketone composite materials of the experimental groups 1 to 4 and the comparative groups 1 to 8 are respectively tested for tensile strength, flexural strength, simply supported beam notched impact strength, and surface resistance performance, and the relevant data are recorded in Table 1.

[0125] Table 1: Test data record table

[0126]

[0127]

[0128] As shown in Table 1, compared with the comparison groups 1 to 8, the polyetheretherketone composite materials prepared in the examples 1 to 4, which use the carbon nanotube composite conductive agent and the modified graphene in combination with the carbon fiber, can not only obtain the characteristic of highly uniform resistance, but also improve the mechanical properties of the composite materials, and have a wide range of applications in the fields of electronics, automobiles, etc.

[0129] The antistatic polyetheretherketone composite material of the invention and its preparation method, by using carbon nanotube composite conductive agent and modified graphene in combination with carbon fiber, optimizing the raw material ratio and processing conditions, adding carbon nanotube composite conductive agent, modified graphene and chopped carbon fiber to polyetheretherketone, taking thermoplastic polyetheretherketone as matrix, carbon nanotube composite conductive agent, modified graphene and chopped carbon fiber as conductive fillers through melt blending, extrusion and granulation, to prepare an antistatic polyetheretherketone composite material with highly uniform resistance while ensuring the excellent performance of PEEK, effectively improving the conductive properties of polyetheretherketone composite material, reducing the risk of static electricity accumulation and discharge, and at the same time, maintaining the original performance advantages of polyetheretherketone material, so that it can still maintain stable performance in an electrostatic environment, suitable for the fields of automobile, electronics and aviation.

[0130] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0131] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. An antistatic polyetheretherketone composite material, characterized in that: The invention is composed of the following raw materials and their weight proportions: 85-100 parts of polyetheretherketone, 1-5 parts of carbon nanotube composite conductive agent, 1-5 parts of carbon fiber and 1-5 parts of modified graphene.

2. The antistatic polyetheretherketone composite material according to claim 1, characterized in that: The melt flow rate of the polyetheretherketone is 5 to 100 g / 10 min.

3. The antistatic polyetheretherketone composite material according to claim 2, characterized in that: The carbon fiber has a chopped length of 2 to 5 mm, a diameter of 7 to 8 μm, and a bulk density of 0.53 to 0.56 g / cm 3 .

4. The antistatic polyetheretherketone composite material according to claim 3, characterized in that: The raw materials of the carbon nanotube composite conductive agent include an amino acid aqueous solution, carbon nanotubes and a conductive filler. The mass fraction of the amino acid in the amino acid aqueous solution is 0.1% to 8%, and the amino acid in the amino acid aqueous solution can form a π-π interaction with the carbon nanotubes. The mass ratio of the amino acid, carbon nanotubes and conductive filler is 0.1 to 10:1 to 35:0 to 15.

5. The antistatic polyetheretherketone composite material according to claim 4, characterized in that: The amino acid is selected from at least one of lysine, phenylalanine and tryptophan, the carbon nanotube is selected from at least one of single-walled carbon nanotube and multi-walled carbon nanotube, and the conductive filler is selected from at least one of carbon black and graphite.

6. The antistatic polyetheretherketone composite material according to claim 5, characterized in that: The raw materials of the modified graphene include graphene, a polymer surfactant, an inorganic salt and carbon black. The graphene is selected from at least one of graphene oxide, thin-layer graphene and multi-layer graphene. The polymer surfactant is selected from at least one of dodecyl polyoxyethylene ether and octanol polyoxyethylene ether. The inorganic salt is selected from at least one of ammonium borate, ammonium nitrate and ammonium carbonate. The carbon black is selected from at least one of acetylene black, Ketjen black and superconducting carbon black.

7. A method for preparing an antistatic polyetheretherketone composite material, characterized in that: An antistatic polyetheretherketone composite material according to any one of claims 1 to 6 is used, comprising the following steps: Ⅰ. Preparation of carbon nanotube composite conductive agent; II. Preparation of modified graphene; III. Accurately weigh each raw material according to its weight ratio; IV. Mixing in a mixer: using a mixer to mix the polyetheretherketone, carbon nanotube composite conductive agent and modified graphene according to the above proportions, and mixing them evenly to obtain a mixed material; V. Use a twin-screw extruder for extrusion granulation. The temperature of each zone of the extruder is set to 320±40℃, the head temperature is 360±20℃, and the speed of the twin-screw extruder is 200-500rpm. After the temperature of each zone of the extruder is stable, the mixed material is fed into the twin-screw extruder from the main feeding port, and the carbon fiber is fed into the twin-screw extruder from the side feeding port; VI. Extrusion granulation: A twin-screw extruder is used to melt-mix the mixture and the carbon fiber, and the mixture is extruded and granulated. The extruded strips are cooled to room temperature and then pelletized to obtain a polyetheretherketone composite material.

8. The method for preparing an antistatic polyetheretherketone composite material according to claim 7, characterized in that: In step I, the following steps are included: A1. Pretreatment: Pretreat the carbon nanotubes and conductive fillers to remove impurities and impurities to ensure that the subsequent modification reaction can proceed smoothly; A2. Introduction of amino acids: Select a suitable amino acid as a modifier and dissolve it in a solvent to obtain an amino acid aqueous solution. Mix the amino acid aqueous solution, carbon nanotubes, and conductive filler according to the mass ratio, stir, and disperse them evenly. A3. Post-reaction treatment: After the reaction is completed, the product is washed, centrifuged and dried to remove unreacted amino acids and solvent residues to obtain a carbon nanotube composite conductive agent.

9. The method for preparing an antistatic polyetheretherketone composite material according to claim 7, characterized in that: In step II, the following steps are included: B1. dissolving a polymer surfactant in a solvent to obtain an aqueous solution of the polymer surfactant, wherein the concentration of the aqueous solution of the polymer surfactant is 3 to 10 mg / ml; B2, adding graphene powder to a polymer surfactant aqueous solution and performing ultrasonic stripping at a rotation speed of 3000-4000 r / min, centrifuging for 20-40 min to obtain a graphene suspension, and then filtering and washing with water to a pH of 7 to obtain pretreated graphene; B3, mixing the pretreated graphene and the inorganic salt in a mass ratio of 1-4:2-8 and grinding for 30 minutes, and then subjecting the mixture to microwave exfoliation for 5-10 minutes at a power of 500-1000 W to obtain layered graphene; B4. Mixing the layered graphene and carbon black in a mass ratio of 5-15:1-5, thermally decomposing the mixture in a muffle furnace under a nitrogen atmosphere at a temperature of 900-1000° C. for 60 min to obtain modified graphene.

Citation Information

Patent Citations

  • Preparation method of high-performance polyetheretherketone-short chopping carbon fiber composite material

    CN106147126A

  • Carbon nano-tube plastic electric-conduction composite material and wet preparation process thereof

    CN110467782A

  • Conductive graphene composite material as well as preparation method and application thereof

    CN110591283A

  • Preparation method of graphene modified polyether-ether-ketone composite material

    CN111171509A

  • Antistatic wafer carrier

    JP1997036216A

Cited By

  • Graphene and carbon nanotube synergistically modified carbon fiber / polyether-ether-ketone composite material and preparation method thereof

    CN122810563A