Anti-oxidation coating for anode of aluminum electrolysis cell and preparation method of anti-oxidation coating

By using activated fly ash, alumina, and quartz sand to form a dense ceramic structural coating, the problem that the anode of the aluminum electrolytic cell is prone to cracking at high temperatures is solved, the service life of the anode is extended, and the utilization rate of fly ash is improved. Achieved efficient antioxidant effect.

CN118772676AActive Publication Date: 2024-10-15CENT SOUTH UNIV

Patent Information

Application Number
CN202410885001.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-15
Estimated Expiration
2044-07-03

AI Technical Summary

Technical Problem

The anti-oxidation coating on the anode of the existing aluminum electrolytic cell is easy to crack at high temperatures, resulting in a shortened service life of the anode, low utilization of fly ash, and environmental pollution.

Method used

Fly ash is used as an inorganic filler, and a high-viscosity alkali metal silicate solution is generated through activation treatment. It is combined with alumina and quartz sand to form a dense ceramic structural coating, which is sprayed on the anode surface to prevent oxidation.

Benefits of technology

It extends the anode service life, reduces the excessive consumption of carbon anodes, reduces anode slag, improves the fluidity and toughness of the coating, reduces the labor intensity of workers, effectively utilizes fly ash, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004925781420000011
    Figure HDA0004925781420000011
  • Figure HDA0004925781420000012
    Figure HDA0004925781420000012
  • Figure HDA0004925781420000021
    Figure HDA0004925781420000021
Patent Text Reader

Abstract

The invention relates to the technical field of electrolytic aluminum, in particular to an anti-oxidation coating for an aluminum electrolysis cell anode and a preparation method of the anti-oxidation coating. The anti-oxidation coating for the anode of the aluminum electrolysis cell comprises 30-55 parts of an inorganic filler, 1-15 parts of a sintering aid, 5-10 parts of a binder and 1-25 parts of a solvent, the inorganic filler contains fly ash; in the inorganic filler, the weight ratio of Al2O3 to SiO2 is 1.0 to 2.0. A high-viscosity alkali metal silicate solution is generated in the activated inorganic filler, silicate is low in melting point and can be molten into a liquid phase at high temperature, and ionic state alkali metal silicate can fill pores among powder and prevent a coating from cracking. Meanwhile, a permeation channel is not reserved for air, and air invasion is prevented. The defects that the conventional ceramic coating is high in sintering temperature, the surface of the coating is not compact enough, pores are reserved and the coating is easy to fall off are overcome, and meanwhile, the use amount of a binder is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum electrolysis, and in particular to an anti-oxidation coating for an anode of an aluminum electrolytic cell and a preparation method thereof. Background Art

[0002] As the "heart" of the aluminum electrolytic cell, the carbon anode is mainly composed of asphalt, petroleum coke, coke and residual anode. Its function is to input direct current into the electrolytic cell during the electrolysis process and participate in the electrochemical reaction in the high-temperature molten salt. In the aluminum electrolysis production process, the carbon anode is in a high-temperature oxidizing atmosphere of 450℃ to 950℃ and a fluorine-containing corrosive atmosphere. Its quality affects the normal production of the electrolytic cell and various production technical indicators, and is closely related to the production cost of primary aluminum.

[0003] During the aluminum electrolysis production process, the anode gas penetrates into the internal pores of the anode to cause Boudol reaction, resulting in secondary consumption; the difference in oxidation between the binder asphalt and the aggregate petroleum coke causes part of the aggregate to fall off and form carbon slag; the huge pressure and flow velocity impact force generated during the movement of the anode bubbles to the edge causes the anode to fall off. Carbon slag will not only shorten the service life of the anode, but also increase the voltage drop, generate heat tanks, and increase the power consumption of aluminum electrolysis. Similarly, removing carbon slag will increase the labor intensity of workers. Therefore, both from an economic perspective and from the perspective of reducing the labor intensity of workers, the quality of anode carbon blocks must be improved.

[0004] There are two main ways to improve the quality of anode carbon blocks in industry: one is to improve the quality of carbon anodes, mainly by using high-quality low-sulfur petroleum coke as raw material. Low-sulfur petroleum coke can not only reduce the slag of anode carbon blocks, but also improve the efficiency of anodes. However, with the development of aluminum electrolysis industry, the demand for high-quality petroleum coke continues to grow, resulting in a reduction in high-quality petroleum coke reserves worldwide. Therefore, this method greatly increases the cost of carbon anodes. Another method is to spray high-temperature anti-oxidation coatings on carbon anodes. Carbon materials begin to oxidize above 500°C. Nanopowder materials are sprayed on the anode surface to form a dense glass phase or ceramic phase below 500°C, isolating the carbon anode from high-temperature gases and reducing excessive consumption of carbon anodes.

[0005] Prior art CN102424730A discloses an anti-oxidation coating for electrolytic aluminum anode carbon blocks and a preparation method thereof. The coating comprises the following components: borax or boric acid, kaolin, industrial phosphoric acid, industrial aluminum sulfate, and water. However, the industrial phosphoric acid in the coating will be dehydrated when heated, causing the coating to crack. Aluminum sulfate will decompose sulfur-containing gas at about 770°C, causing harm to the environment.

[0006] Prior art CN104005056A discloses a method for preparing an electrolytic aluminum carbon anode protective coating, which uses calcium aluminate cement as a binder, waste electrolyte from aluminum electrolysis production as aggregate, and sodium pyrophosphate, sodium tripolyphosphate, sodium hexametaphosphate, sodium lignin sulfonate, calcium lignin sulfonate, etc. as admixtures. However, the coating has a complex composition, and the admixtures used contain carbon-containing organic matter, which is easily volatilized at high temperatures and causes cracking of the coating.

[0007] Prior art CN 113563056 B proposes a coating material for high-temperature oxidation protection of carbon anodes, which is composed of the following components: 35-55wt% inorganic binder, 30-60wt% composite ceramic filler, 1-10wt% catalyst, 0-1wt% sintering agent and 1-10wt% toughening agent. The coating material of the invention has good toughness, strong bonding force and strong thermal shock resistance, and is easy to construct, solidifies at room temperature, densifies at low temperature, is non-toxic and environmentally friendly, and is durable and effective. It can significantly reduce the high-temperature oxidation and burning of carbon anodes and extend the service life of the anode. However, the coating relies on low-temperature sintering of the coating components to form a ceramic structure to resist oxidation by air. The micro-liquid phase in the coating is difficult to fill the ceramic pores, resulting in a non-dense structure. The reserved ceramic pores provide a channel for air oxidation, which can easily cause partial oxidation of the anode substrate.

[0008] Fly ash is a solid waste discharged during the combustion process of coal-fired power plant boilers. It is composed of fine particles discharged from the flue gas duct and collected after the inorganic minerals in the raw materials undergo a series of physical and chemical changes such as burning, conversion, melting, and cooling after the coal powder or coal sludge is burned at high temperature in the furnace. Its main components are SiO2 and Al2O3, accounting for 60-90% of the total amount, and there are also small amounts of Fe2O3, CaO, MgO, K2O, and Na2O. The comprehensive utilization of fly ash has basically gone through three development stages: "mainly based on stockpiling - storage and utilization combined - mainly based on utilization". Although the annual utilization rate of fly ash has reached more than 70%, due to the long-term accumulation, the stockpiling surplus of fly ash is still large, with a total accumulation of more than 2.5 billion tons, and it is still increasing year by year, which has brought serious impacts on the environment. At present, the utilization of fly ash is mainly concentrated in building products, construction projects, road projects, etc. However, due to the high content of impurities in fly ash and the difficulty of pretreatment, the utilization rate still needs to be further increased. Summary of the invention

[0009] The purpose of the present invention is to provide an anti-oxidation coating for an aluminum electrolytic cell anode to enhance the service life of an aluminum electrolytic anode carbon block.

[0010] In order to achieve the above object, the technical solution of the present invention is as follows:

[0011] An anti-oxidation coating for an aluminum electrolytic cell anode, comprising, by weight: 30-55 parts of an inorganic filler, 1-15 parts of a sintering aid, 5-10 parts of a binder and 1-25 parts of a solvent;

[0012] The inorganic filler contains fly ash;

[0013] In the inorganic filler, the weight ratio of Al2O3 to SiO2 is 1.0-2.0.

[0014] The only components of the anti-oxidation coating for aluminum electrolytic cell anodes are Al2O3 and SiO2. The weight ratio of Al2O3 and SiO2 in the coating determines the anti-oxidation performance of the coating. SiO2 determines the fluidity of the coating. SiO2 forms a high-viscosity liquid phase at high temperatures. When cracks or bubbles appear in the coating, the flowing liquid phase can heal the cracks and bubbles to ensure that the coating will not break. When m(SiO2) is small, the cracks in the coating are difficult to heal. Al2O3 forms a solid phase at high temperatures, which determines the toughness of the coating. If m(Al2O3) is too small, the coating will easily flow freely on the anode surface, exposing the inner carbon anode. The coating has the best protective effect when the weight ratio of Al2O3 and SiO2 is 1.0-2.0. When the weight ratio of Al2O3 and SiO2 is greater than 2, m(Al2O3) is too large, the fluidity of the coating is reduced, and cracks in the coating are difficult to heal. When the weight ratio of Al2O3 and SiO2 is less than 1, m(Al2O3) is too small, the fluidity of the coating is too large, and it flows on the anode surface, exposing the carbon anode substrate.

[0015] The present invention utilizes the characteristics of high aluminum and high silicon in fly ash, uses fly ash as a filler, and prepares a new type of antioxidant coating for the anode of aluminum electrolysis cell. On the one hand, it reduces the inventory of fly ash and provides a new idea for the rational use of this solid waste; on the other hand, it can effectively reduce the excessive consumption of carbon anodes, reduce the slagging of anode carbon blocks, extend the service life of aluminum electrolysis anode carbon blocks, and reduce the labor intensity of workers.

[0016] In a preferred embodiment, the inorganic filler is an activated inorganic filler.

[0017] The reasons for activation are as follows:

[0018] 1. The activated components are fly ash and alkali metal. Before activation, the two components are not sticky and cannot be bonded to the coating surface, and will crack. After activation, the two components can be bonded to the coating surface;

[0019] 2. The principle of activation is that the silicon dioxide in fly ash dissolves under alkaline conditions to generate high-viscosity alkali metal silicates such as sodium silicate and potassium silicate (inorganic polymer materials). The solubility of silicon dioxide is related to the activation temperature and pressure. The higher the activation temperature and the greater the pressure, the higher the solubility of silicon dioxide and the larger the prepared binder.

[0020] 3. During the activation process, the silica powder dissolves and turns into ions in the solution. The two are completely dissolved and mixed. After the inorganic filler is air-dried, no pores will be left, forming a dense surface structure.

[0021] In one preferred embodiment, the activation step of the inorganic filler comprises:

[0022] S1, wet-grinding the inorganic filler to obtain a slurry;

[0023] S2. Activate the slurry for 1.5-5h at a pressure of not less than 0.6MPa, a temperature of not less than 160°C, and a stirring rate of 15-80 rpm to obtain an activated inorganic filler.

[0024] The activation principle is as follows:

[0025] 1. Activation The first step is wet grinding to obtain slurry, the purpose is to reduce the particle size of the powder material. The smaller the particle size, the larger the specific surface area, the faster the dissolution rate in the alkali solution, and the more fully dissolved. Without wet grinding, the powder particle size is large, the dissolution rate is slow, or it is basically insoluble.

[0026] 2. Activation is to dissolve silica and increase its activity. Insoluble silica is a powder and has no viscosity. The prepared coating is very easy to crack at room temperature.

[0027] If the activation pressure and temperature are too low, and the time is too short, less SiO2 will be dissolved, the fluidity will be low, the coating viscosity will be low, and the protective performance will be poor; if the temperature is too high, the pressure is too high, and the time is too long, there will be too much SiO2, the coating's melting point will be low, and the fluidity will be strong at high temperatures, which will reduce the coating's protective performance.

[0028] In one of the preferred embodiments, in step S2, the slurry is activated at an activation pressure of 0.6-0.8 MPa and an activation temperature greater than 160-180°C.

[0029] In one preferred embodiment, the fly ash includes 30-70 parts of Al2O3, 10-30 parts of quartz sand, 0-12 parts of calcium oxide, 0-2 parts of magnesium oxide and 0-10 parts of volatile matter.

[0030] In one preferred embodiment, the inorganic filler further includes one or both of alumina and quartz sand.

[0031] The system of the present invention can only include alumina and quartz sand. Other materials such as silicon dioxide powder have high water absorption, are easy to dry, and cannot be sprayed.

[0032] By adding alumina and quartz sand, the addition amounts of alumina, fly ash and quartz sand in the system are controlled so that the weight ratio of Al2O3 to SiO2 in the composition is 1.0-2.0.

[0033] In one preferred embodiment, the inorganic filler includes 30-60 parts of fly ash and 2-20 parts of alumina.

[0034] In one preferred embodiment, the inorganic filler includes 30-60 parts of fly ash and 2-20 parts of quartz sand.

[0035] In a preferred embodiment, the sintering aid is potassium chloride.

[0036] There are two reasons for adding potassium chloride: 1. Potassium feldspar formed by potassium and SiO2 and Al2O3 at high temperature has high viscosity, which bonds the coating to the surface of the carbon anode; 2. Potassium chloride has a low melting point and can melt at a lower temperature to fill the pores and cracks in the middle of the solid coating and protect the carbon anode substrate. The temperature of KF is too high and cannot fill the pores and cracks between the coatings in time at low temperatures, which will lead to increased mass loss of the carbon anode.

[0037] In a preferred embodiment, the binder is sodium silicate.

[0038] In a preferred embodiment, the solvent is one or more of water, ethanol, methanol, and ethylene glycol monobutyl ether, preferably water, which has higher safety.

[0039] The present invention also claims a method for preparing the anti-oxidation coating for the anode of the aluminum electrolytic cell, comprising:

[0040] A solvent is added to the activated inorganic filler to disperse it; and then a sintering aid and a binder are added to obtain the anti-oxidation coating for the anode of the aluminum electrolytic cell.

[0041] An anti-oxidation coating for an aluminum electrolytic cell anode, the preparation method of which is as follows: spraying the anti-oxidation coating for an aluminum electrolytic cell anode on the surface of a carbon anode with a thickness controlled at 0.2 to 0.8 μm, drying naturally for 24 to 48 hours, and reacting at 800 to 1100° C. for 5 to 12 hours to obtain the coating.

[0042] The coating material of the present invention only needs to be sprayed on the surface of the carbon anode with a thickness of 0.2-0.8 μm, and then naturally dried for 24-48 hours and reacted at 800-1100° C. for 5-12 hours before use, which can extend the anode cycle by two days.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] (1) A high-viscosity alkali metal silicate solution is generated in the activated inorganic filler of the present invention. The melting point of silicate is low and it can be melted into a liquid phase at high temperature. The ionic alkali metal silicate can fill the pores between the powders to prevent the coating from cracking. At the same time, no channel is reserved for air to penetrate, blocking the invasion of air. It overcomes the shortcomings of the previous coating ceramic coating, such as high sintering temperature, insufficient density of the coating surface, pores, and easy falling off, while reducing the cost of the coating. The activated alkali metal silicate is a silicate structure with silicon-oxygen tetrahedron as the backbone. After the structure is formed, aluminum oxide will replace part of the silicon-oxygen tetrahedron to form an aluminosilicate structure. The viscosity of the aluminosilicate is higher after high-temperature melting, and it will form a dense structure similar to the ceramic surface glaze layer to prevent air from corroding the carbon anode.

[0045] (2) The present invention adds a sintering aid to reduce the sintering temperature of the filler, so that the filler is sintered between 500°C and 600°C to form a dense ceramic structure, and the anodization rate can be effectively reduced at a temperature above 600°C.

[0046] (3) The present invention uses activated fly ash as the coating raw material, exploring a new path for rationally utilizing fly ash and reducing solid waste accumulation. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 is the oxidation result of the sample in Example 1;

[0048] Figure 2 It is the oxidation result of the sample of comparative example 1;

[0049] Figure 3 It is the oxidation result of the sample of comparative example 2;

[0050] Figure 4 It is the oxidation result of the sample in Example 2;

[0051] Figure 5 It is the oxidation result of the sample of comparative example 3;

[0052] Figure 6 It is the oxidation result of the sample in Example 3;

[0053] Figure 7 is the microscopic morphology of the coating of Example 3;

[0054] Figure 8 This is the XRD phase result of the coating in Example 3. DETAILED DESCRIPTION

[0055] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0056] Example 1

[0057] The specific implementation steps of this embodiment are as follows:

[0058] (1) Fly ash from a place in Inner Mongolia was selected, and its composition is as follows:

[0059] <![CDATA[Al2O3]]> <![CDATA[SiO2]]> <![CDATA[Fe2O3]]> CaO MgO Loss on ignition 44.74% 31.91% 4.17% 9.77% 0.58% 6.19%

[0060] (2) 30 parts by mass of fly ash, 20 parts by mass of alumina, and 20 parts by mass of water were placed in a sand mill and wet-milled for 5-12 hours, at which point the Al2O3:SiO2 content of the filler was ≈2:1;

[0061] (3) adding the wet-milled slurry into an autoclave and subjecting it to activation treatment for 3 h at 0.6 MPa, 160° C., and a stirring rate of 50 rpm;

[0062] (4) The filler in step (3) is added to a high-speed disperser, and 10 parts of sodium silicate and 5 parts of potassium chloride are added to the disperser, and dispersed at a speed of 200 rpm for 1 to 2 hours to obtain coating 1.

[0063] (5) The addition of 20 parts of alumina in step (2) is then replaced by adding 10 parts of alumina and 5 parts of alumina. At this time, the Al2O3:SiO2 in the filler is 1.5:1 and 1:1 respectively. The other steps, raw materials and processes are the same as above, and coating 2 and coating 3 are obtained respectively.

[0064] (6) The prepared coating 1-3 was sprayed onto the surface of a 6×6×1 cm carbon anode with a film thickness of 0.4 to 0.6 μm. After drying at room temperature for 48 h, it was placed in a muffle furnace and reacted at 950°C for 10 h. After oxidation, the samples were all as shown in Figure 1 The carbon anodization results of coating 2 are shown in Table 1. The carbon anodization results of coatings 1 and 3 are close to those of coating 2.

[0065] Comparative Example 1

[0066] Fly ash from a place in Inner Mongolia was selected, and 14 parts of quartz sand powder were added instead of 20 parts of alumina in step (2) of Example 1. At this time, the Al2O3:SiO2 content in the filler was 0.5:1, and the other steps, raw materials and processes were the same as those in Example 1. Figure 2 , the carbon anodization results are shown in Table 1.

[0067] Comparative Example 2

[0068] Fly ash from a place in Inner Mongolia was selected, and the addition of 20 parts of alumina in step (1) of Example 1 was changed to adding 16 parts of alumina powder. At this time, the Al2O3:SiO2 in the filler was ≈3:1, and the other steps, raw materials and processes were the same as in Example 1. Figure 3 , the carbon anodization results are shown in Table 1.

[0069] Comparing Example 1 with Comparative Examples 1-2, the Al2O3:SiO2≈1-2:1 ratio in Example 2 has the best protection effect.

[0070] Example 2

[0071] The specific implementation steps of this embodiment are as follows:

[0072] (1) Fly ash from a place in Inner Mongolia was selected, and its composition is as follows:

[0073]

[0074]

[0075] (2) 30 parts by mass of fly ash, 10 parts by mass of alumina, and 20 parts by mass of water were placed in a sand mill and wet-milled for 5-12 hours, at which point the Al2O3:SiO2 content of the filler was ≈1.5:1;

[0076] (3) adding the wet-milled slurry into an autoclave and subjecting it to activation treatment for 3 h at 0.8 MPa, 180° C., and a stirring rate of 50 rpm;

[0077] (4) The filler in step (3) is added to a high-speed disperser, and 10 parts of sodium silicate and 5 parts of potassium chloride are added to the disperser, and dispersed at a speed of 200 rpm for 1 to 2 hours to obtain coating 4.

[0078] (5) The prepared coating 4 was sprayed onto the surface of a 6×6×1 cm carbon anode with a film thickness of 0.4 to 0.6 μm. After drying at room temperature for 48 h, it was placed in a muffle furnace and reacted at 950°C for 10 h. After oxidation, the sample was Figure 4 , the carbon anodization results are shown in Table 1.

[0079] Comparing coating 2 and coating 4, increasing the activation temperature to 180°C and the pressure to 0.8 MPa has no effect on the protective properties of the coating.

[0080] Comparative Example 3

[0081] Example 2 was repeated, except that the pressure in step (3) of Example 2 was changed to 0.3 MPa and the temperature was changed to 130°C. The other steps, raw materials and processes were the same as those of Example 2. Figure 5 , the carbon anodization results are shown in Table 1.

[0082] Comparative Example 4

[0083] Example 2 was repeated, except that the pressure in step (3) of Example 2 was changed to 0.9 MPa and the temperature was changed to 190° C. The other steps, raw materials and processes were the same as Example 2. The carbon anodization results are shown in Table 1.

[0084] Comparative Examples 1, 2 and Comparative Examples 3-4, when the activation pressure is lower than 0.6 MPa and the activation temperature is lower than 160°C, the protective performance of the coating will be reduced. When the activation pressure is higher than 0.8 MPa and the activation temperature is higher than 180°C, the protective performance of the coating will be reduced. The optimal activation conditions are an activation pressure of 0.6-0.8 MPa, an activation temperature greater than 160-180°C, and an activation treatment of 2 hours at a stirring rate of 50 rpm.

[0085] Example 3

[0086] Fly ash from a place in Heilongjiang was selected, and its composition is as follows:

[0087] <![CDATA[Al2O3]]> <![CDATA[SiO2]]> <![CDATA[Fe2O3]]> CaO MgO Loss on ignition 20.70% 61.15% 4.75% 3.60% 0.86% 4.60%

[0088] (1) 20 parts by mass of fly ash, 25 parts by mass of alumina, and 20 parts by mass of water were placed in a sand mill and wet-milled for 5-12 hours, at which point the Al2O3:SiO2 content of the filler was ≈1.5:1;

[0089] (2) adding the wet-milled slurry into an autoclave and subjecting it to activation treatment for 2 to 5 hours at 0.6 MPa, 170° C., and a stirring rate of 50 rpm;

[0090] (3) The filler in step (3) is added to a high-speed disperser, and 10 parts of sodium silicate and 5 parts of potassium chloride are added to the disperser, and dispersed at a speed of 200 rpm for 1 to 2 hours.

[0091] (4) The prepared coating was sprayed onto the surface of a 6×6×1 cm carbon anode, dried at room temperature for 48 h, and then placed in a muffle furnace and reacted at 950°C for 10 h. After oxidation, the sample was Figure 6 The carbon anodization results are shown in Table 1. The microstructure of the coating is shown in Figure 7 , XRD results are as follows Figure 8 .

[0092] By comparing Examples 2 and 3, it can be found that fly ash from different regions does not affect the anti-oxidation performance of the coating. The main factor affecting the anti-oxidation performance is the mass ratio of Al2O3 and SiO2. The best anti-oxidation effect is achieved when Al2O3:SiO2 is 1.0-2.0:1. At the same time, the activation conditions in the coating preparation process have a greater impact on the anti-oxidation performance. After the coating filler is wet-ground and enters the autoclave, when the activation pressure exceeds 0.6MPa, the anti-oxidation performance of the coating is no longer affected.

[0093] By comparing Example 2 and Example 3, it can be found that fly ash produced by different enterprises from different origins can be used to prepare the antioxidant coating. Therefore, this method is generally applicable to the treatment of fly ash.

[0094] Comparative Example 5

[0095] Example 3 was repeated, except that 5 parts of potassium chloride were added in step (3) of Example 3 instead of 5 parts of potassium fluoride. The carbon anodization results are shown in Table 1.

[0096] Comparative Example 6

[0097] Example 3 was repeated, except that 5 parts of sodium chloride were added instead of 5 parts of potassium chloride in step (3) of Example 3. The carbon anodization results are shown in Table 1.

[0098] Comparative Example 3 and Comparative Example 5, since the melting point of chloride is lower than that of potassium fluoride, a liquid phase can be formed at a relatively low temperature to seal the pores in the coating and prevent air from entering, thus providing a strong protective effect.

[0099] Comparing Example 3 with Comparative Example 6, since potassium ions enter the coating to form potassium feldspar with higher viscosity, the bonding force between the coating and the carbon anode is increased, so the protection effect is good.

[0100] Example 4

[0101] Fly ash from a place in Heilongjiang was selected, and its composition is as follows:

[0102] <![CDATA[Al2O3]]> <![CDATA[SiO2]]> <![CDATA[Fe2O3]]> CaO MgO Loss on ignition 60.70% 20.15% 4.75% 3.60% 0.86% 4.60%

[0103] (1) 20 parts of fly ash, 4 parts of quartz sand, and 20 parts of water were wet-milled in a sand mill for 5-12 hours, at which point the Al2O3:SiO2 ratio in the filler was ≈1.5:1;

[0104] (2) adding the wet-milled slurry into an autoclave and subjecting it to activation treatment for 2 to 5 hours at 0.6 MPa, 170° C., and a stirring rate of 50 rpm;

[0105] (3) The filler in step (3) is added to a high-speed disperser, and 10 parts of sodium silicate and 5 parts of potassium chloride are added to the disperser, and dispersed at a speed of 200 rpm for 1 to 2 hours.

[0106] (4) The prepared coating was sprayed onto the surface of a 6×6×1 cm carbon anode, dried at room temperature for 48 h, and then placed in a muffle furnace and reacted at 950°C for 10 h. The carbon anode oxidation results are shown in Table 1.

[0107] Comparative Example 7

[0108] Example 4 was repeated, except that steps (1) and (2) of Example 4 were replaced by not adding activated inorganic materials, and 20 parts of fly ash, 4 parts of quartz sand, and 20 parts of water were directly added to a high-speed disperser, mixed with 10 parts of sodium silicate and 5 parts of potassium chloride, and other raw materials, processes and steps were the same as Example 4. The prepared coating was sprayed onto the surface of a 6×6×1 cm carbon anode, dried at room temperature for 48 hours, and then placed in a muffle furnace and reacted at 950°C for 10 hours. The carbon anode oxidation results are shown in Table 1.

[0109] Comparative Example 8

[0110] Example 4 was repeated, except that the slurry after wet grinding in step (1) of Example 4 was directly added to a high-speed disperser and mixed with 10 parts of sodium silicate and 5 parts of potassium chloride. The other raw materials, processes and steps were the same as those of Example 4. The prepared coating was sprayed onto the surface of a 6×6×1 cm carbon anode, dried at room temperature for 48 hours, and then placed in a muffle furnace and reacted at 950° C. for 10 hours. The carbon anode oxidation results are shown in Table 1.

[0111] Comparative Example 9

[0112] Example 4 was repeated, except that 20 parts of fly ash, 4 parts of quartz sand, and 20 parts of water in Example 4 were simply stirred and mixed, then added to an autoclave, and activated for 2 to 5 hours at 0.6 MPa, 170°C, and a stirring rate of 50 rpm; other raw materials, processes, and steps were the same as in Example 4. The prepared coating was sprayed onto the surface of a 6×6×1 cm carbon anode, dried at room temperature for 48 hours, and then placed in a muffle furnace for reaction at 950°C for 10 hours. The carbon anode oxidation results are shown in Table 1.

[0113] Comparing Example 4 with Comparative Example 7, in Comparative Example 7, unactivated fly ash is added to the coating, the content of sodium silicate in the coating is low, the coating viscosity is low, and it cannot be effectively bonded to the surface of the carbon anode. In addition, the high melting point of alumina and silicon dioxide reduces the liquid content of the coating, which eventually leads to the failure of the coating and the maximum weight loss of the carbon anode.

[0114] Comparing Example 4 and Comparative Example 8, in Comparative Example 8, inorganic fillers that have only been wet ground are added to the coating. Although the particle size of the inorganic filler is appropriate, since it has not been activated at high temperature, the silica dissolves and increases its activity, and the undissolved silica is a powder and has no viscosity. The prepared coating is very easy to crack at room temperature.

[0115] Comparing Example 4 with Comparative Example 9, in Comparative Example 9, inorganic fillers that were directly activated at high temperature without wet grinding were added to the coating. Although the particle size of the inorganic filler was not suitable, the dissolution rate was slow, or it was basically insoluble, resulting in coating failure.

[0116] Table 1 Graphite oxidation results obtained in different embodiments and comparative examples

[0117] Example Graphite mass / g Coating mass after drying / g Mass after oxidation / g Quality loss Example 1 51.65 55.38 48.96 11.59% Comparative Example 1 52.47 55.88 43.28 22.54% Comparative Example 2 53.12 56.47 39.39 30.25% Example 2 49.94 52.89 49.00 7.35% Comparative Example 3 49.05 52.20 45.65 12.54% Comparative Example 4 50.41 54.23 45.80 15.54% Example 3 48.90 52.04 48.44 7.21% Comparative Example 5 49.77 53.05 44.90 15.36% Comparative Example 6 51.43 55.42 48.48 12.53% Example 4 50.88 53.42 49.31 7.69% Comparative Example 7 49.99 53.65 7.09 86.78% Comparative Example 8 52.49 55.86 8.14 85.42% Comparative Example 9 51.56 54.29 10.54 80.59%

[0118] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An anti-oxidation coating for an aluminum electrolytic cell anode, characterized in that: include: 30-55 parts of inorganic filler, 1-15 parts of sintering aid, 5-10 parts of binder and 1-25 parts of solvent; The inorganic filler contains fly ash; In the inorganic filler, the weight ratio of Al2O3 to SiO2 is 1.0-2.

0.

2. The anti-oxidation coating for aluminum electrolytic cell anode according to claim 1, characterized in that: The inorganic filler is an activated inorganic filler; preferably, the activation step of the inorganic filler comprises: S1, wet-grinding the inorganic filler to obtain a slurry; S2. Activate the slurry for 1.5-5h at a pressure of not less than 0.6MPa, a temperature of not less than 160°C, and a stirring rate of 15-80 rpm to obtain an activated inorganic filler.

3. The anti-oxidation coating for aluminum electrolytic cell anode according to claim 2, characterized in that: In the step S2, the slurry is activated at an activation pressure of 0.6-0.8 MPa and an activation temperature greater than 160-180°C.

4. The anti-oxidation coating for aluminum electrolytic cell anode according to claim 1, characterized in that: The fly ash comprises 30-70 parts of Al2O3, 10-30 parts of quartz sand, 0-12 parts of calcium oxide, 0-2 parts of magnesium oxide and 0-10 parts of volatile matter.

5. The anti-oxidation coating for aluminum electrolytic cell anode according to claim 1, characterized in that: The inorganic filler also includes one or two of alumina and quartz sand.

6. The anti-oxidation coating for aluminum electrolytic cell anode according to claim 1, characterized in that: The sintering aid is potassium chloride.

7. The anti-oxidation coating for aluminum electrolytic cell anode according to claim 1, characterized in that: The binder is sodium silicate.

8. The anti-oxidation coating for aluminum electrolytic cell anode according to claims 1-7, characterized in that: The solvent is one or more of water, ethanol, methanol, and ethylene glycol monobutyl ether.

9. The method for preparing the anti-oxidation coating for the anode of the aluminum electrolysis cell according to claims 1-8, characterized in that: include: Adding a solvent to the activated inorganic filler to disperse it; Then, a sintering aid and a binder are added to obtain the anti-oxidation coating for the anode of the aluminum electrolytic cell.

10. An anti-oxidation coating for an aluminum electrolytic cell anode, the preparation method of which is as follows: spraying the anti-oxidation coating for an aluminum electrolytic cell anode according to claims 1-8 on the surface of a carbon anode with a thickness controlled at 0.2-0.8 μm, drying naturally for 24-48 hours, and reacting at 800-1100°C for 5-12 hours to obtain the anti-oxidation coating.

Citation Information

Patent Citations

  • Preparation method of high-temperature chlorine corrosion resistant ceramic coating with fly ash as base material for incinerator

    CN114736003A

  • Semi-internal combustion type solid waste-based ceramic flat sheet membrane and preparation method thereof

    CN116328555A

  • Aluminum electrolysis anode ceramic-based antioxidant coating and preparation method thereof

    CN117701045A

  • Sprayable phosphate cementitious coatings and a method and apparatus for the production thereof

    US20020009622A1

  • Thermal protective coating

    US20060156958A1

Cited By

  • Multifunctional binder for aluminum electrolysis, preparation method therefor and use thereof

    WO2026188664A1