High temperature resistant fire retardant coating powder and preparation method thereof
By using phenolic epoxy resin, bisphenol A epoxy resin and modified nano alumina agent in powder fire-retardant coatings, the problem of poor wear resistance and adhesion of powder fire-retardant coatings under high temperature conditions is solved. , achieving improved stability under acid corrosion and ultraviolet light.
Patent Information
- Application Number
- CN202411172343.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing powdered fire-retardant coatings have poor wear resistance and adhesion under high temperature conditions, and their stability is reduced under acid corrosion and ultraviolet light, making it difficult to achieve coordinated improvements in high temperature resistance, wear resistance and adhesion.
Using phenolic epoxy resin, bisphenol A type epoxy resin, special functional phase modulator, modified nano alumina agent, etc., high-temperature fire-resistant coating powder is prepared through heat treatment, stirring, ball milling and other processes to improve its wear resistance , adhesion and stability.
It significantly improves the wear resistance, adhesion and high temperature stability of the product, enhances the stability under acid corrosion and ultraviolet light conditions, and achieves coordinated improvements in high temperature resistance, wear resistance and adhesion.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fire retardant coating powder, and in particular to high temperature resistant fire retardant coating powder and a preparation method thereof. Background Art
[0002] Fire retardant coating is a special coating used on the surface of combustible substrates to reduce the flammability of the coated material surface, block the rapid spread of fire, and improve the fire resistance limit of the coated material. Powder-type fire retardant coatings have poor high temperature resistance and are prone to cracking under high temperature conditions. At the same time, the wear resistance and adhesion of the product are poor. It is difficult for the product to achieve coordinated improvements in wear resistance, adhesion and high temperature resistance. In addition, the product's stability is reduced under acid corrosion and UV weathering conditions, further limiting the product's use efficiency. Summary of the invention
[0003] In view of the defects of the prior art, the purpose of the present invention is to provide a high temperature resistant fire retardant coating powder and a preparation method thereof to solve the problems raised in the above background technology.
[0004] The present invention solves the technical problem by adopting the following technical solution:
[0005] The present invention provides a high temperature resistant fire retardant coating powder, comprising the following raw materials in parts by weight:
[0006] 35-45 parts of phenolic epoxy resin, 15-25 parts of bisphenol A epoxy resin with epoxy equivalent of 1000, 10-15 parts of special functional phase modifier, 8-12 parts of curing agent, 5-8 parts of modified nano alumina agent, 4-7 parts of flame retardant, 2-3 parts of antioxidant and 2-3 parts of dispersant.
[0007] Preferably, the high temperature resistant fire retardant coating powder comprises the following raw materials in parts by weight:
[0008] 40 parts of phenolic epoxy resin, 20 parts of bisphenol A epoxy resin with epoxy equivalent of 1000, 12.5 parts of special functional phase modifier, 10 parts of curing agent, 6.5 parts of modified nano alumina agent, 5.5 parts of flame retardant, 2.5 parts of antioxidant and 2.5 parts of dispersant.
[0009] Preferably, the flame retardant is magnesium hydroxide; the dispersant is calcium stearate; the antioxidant is pentaerythritol dioctadecyl diphosphite; and the curing agent is 2-phenylimidazole.
[0010] Preferably, the preparation method of the special functional phase modifier is:
[0011] S01: heat-treat the nano-bentonite at 300-350°C for 10-20 min, then cool to 55°C at a rate of 2-5°C / min and keep warm;
[0012] 4-7 parts of the insulated nano-bentonite are added to 8-12 parts of a phosphate buffer solution with a pH value of 5.5, and then 2-3 parts of nano-silica sol and 1-3 parts of a sodium citrate solution with a mass fraction of 4-6% are added for stirring, and then washed with water and dried to obtain a nano-bentonite conditioner;
[0013] S02: immersing the silicon carbide whisker in a yttrium nitrate solution of 4 to 7 times the total amount of the silicon carbide whisker, immersing the solution fully, with an immersion power of 350 to 400 W, immersing for 20 to 30 minutes, and completing the immersion to obtain a modified yttrium silicon carbide whisker agent;
[0014] S03: Mix 1-3 parts of silane coupling agent KH550, 2-4 parts of carboxymethyl cellulose and 2-5 parts of sodium alginate solution to obtain a compatibilizing agent;
[0015] Add the phase agent to the modified yttrium silicon carbide whisker agent in a weight ratio of 2:5 and continue to mix well to obtain a phase-adjusted silicon carbide whisker agent;
[0016] S04: The phase-adjusting silicon carbide whisker agent and nano-bentonite regulator are mixed in a weight ratio of 3:5 and ball-milled at a ball-milling speed of 1000 r / min for 1 to 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a special functional phase-adjusting agent.
[0017] Preferably, the mass fraction of the sodium alginate solution is 4-7%; the mass fraction of the yttrium nitrate solution is 2-5%; the rotation speed of the stirring treatment is 550-750 r / min, and the stirring time is 35-45 min.
[0018] Preferably, the preparation method of the modified nano alumina agent is:
[0019] S11: irradiating the nano-alumina in a proton irradiation box for 10-15 minutes at an irradiation power of 350-400W, and obtaining irradiated nano-alumina after the irradiation is completed;
[0020] The irradiated nano-alumina, sodium silicate solution and lanthanum chloride solution are mixed in a weight ratio of (2-5): (4-7): 2 to obtain a nano-alumina modified solution;
[0021] S12: The nano-alumina modified liquid and the performance-adjusting agent doped with aluminum silicate fiber are mixed in a weight ratio of (5-7):3 and ball-milled at a speed of 1500-2000 r / min for 1 hour. After the ball milling is completed, the mixture is washed with water and dried to obtain a modified nano-alumina agent.
[0022] Preferably, the mass fraction of the sodium silicate solution is 2-5%; the mass fraction of the lanthanum chloride solution is 3-6%.
[0023] Preferably, the preparation method of the performance-adjusting agent doped with aluminum silicate fiber is:
[0024] 4-7 parts of aluminum silicate fiber and 1-3 parts of silane coupling agent KH560 are added to 5-8 parts of chitosan solution, and then 2-4 parts of hydroxyapatite and 2-3 parts of sodium dodecylbenzene sulfonate are added and blended for ultrasonic treatment at an ultrasonic power of 400-500 W for 30-40 minutes. After the ultrasonic treatment is completed, the mixture is washed with water and dried to obtain a performance-enhancing agent doped with aluminum silicate fiber.
[0025] Preferably, the mass fraction of the chitosan solution is 2-5%.
[0026] The present invention also provides a method for preparing high temperature resistant fire retardant coating powder, comprising the following steps:
[0027] The raw materials are weighed according to weight, mixed, and then sent into a twin-screw extruder for extrusion at an extrusion temperature of 90-95°C and an extrusion speed of 450-500r / min to obtain an extrudate, which is then ground through 200 meshes to obtain a high-temperature resistant fire-retardant coating powder.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The high temperature resistant fireproof coating powder of the present invention adopts phenolic epoxy resin and bisphenol A epoxy resin with an epoxy equivalent of 1000 as a base material, and improves the functional effect of the product by adding a curing agent, a flame retardant, an antioxidant and a dispersant as functional additives to adjust the base material, and the added special functional phase adjusting agent and modified nano alumina agent are used as coordination raw materials. Through the mutual coordination and synergy of the two, the wear resistance, adhesion and high temperature resistance of the product are coordinated and improved, and the product has a significant stability effect under acid corrosion and ultraviolet weathering conditions; the special functional phase adjusting agent is Nano bentonite was heat treated at 300-350°C for 10-20 min, and then cooled to 55°C at a rate of 2-5°C / min to optimize the activity of nano bentonite. The dispersion and activity of nano bentonite were further optimized by stirring with phosphate buffer solution, nano silica sol and 4-6% sodium citrate solution by mass fraction, so as to better coordinate with the phase-adjusted silicon carbide whisker agent. The phase-adjusted silicon carbide whisker agent used silicon carbide whiskers immersed in yttrium nitrate solution to optimize the activity of the whiskers, and the whisker-like structure of the silicon carbide whiskers was distributed. In the system, the lamellar nano-bentonite is better coordinated to optimize the performance coordination of the system. At the same time, the silane coupling agent KH550, carboxymethyl cellulose and sodium alginate solution are mixed to fully obtain the phase agent. The addition of the phase agent further enhances the interface effect between the raw materials, improves the coordination effect between the raw materials, and further improves the performance of the product; the modified nano-alumina agent uses nano-alumina to be irradiated in the proton irradiation box before, optimizes the active efficiency of nano-alumina, and adopts sodium silicate solution and lanthanum chloride solution to coordinate and improve the nano-alumina and The synergistic effect of the conditioning agent doped with aluminum silicate fiber. The conditioning agent doped with aluminum silicate fiber uses aluminum silicate fiber as the needle-like structure, and is matched with silane coupling agent KH560, chitosan solution and sodium dialkylbenzene sulfonate to enhance the coordination and harmonization effect between the raw materials. At the same time, the added hydroxyapatite further enhances the coordinated aluminum silicate fiber, improves the coordinated synergistic effect of the conditioning agent doped with aluminum silicate fiber and nano-alumina, further improves the wear resistance, adhesion and high temperature resistance of the product, and further improves the stability of the product under acid corrosion and UV weathering conditions. DETAILED DESCRIPTION
[0030] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] A high temperature resistant fire retardant coating powder of this embodiment includes the following raw materials in parts by weight:
[0032] 35-45 parts of phenolic epoxy resin, 15-25 parts of bisphenol A epoxy resin with epoxy equivalent of 1000, 10-15 parts of special functional phase modifier, 8-12 parts of curing agent, 5-8 parts of modified nano alumina agent, 4-7 parts of flame retardant, 2-3 parts of antioxidant and 2-3 parts of dispersant.
[0033] The high temperature resistant fire retardant coating powder of this embodiment includes the following raw materials in parts by weight:
[0034] 40 parts of phenolic epoxy resin, 20 parts of bisphenol A epoxy resin with epoxy equivalent of 1000, 12.5 parts of special functional phase modifier, 10 parts of curing agent, 6.5 parts of modified nano alumina agent, 5.5 parts of flame retardant, 2.5 parts of antioxidant and 2.5 parts of dispersant.
[0035] The flame retardant of this embodiment is magnesium hydroxide; the dispersant is calcium stearate; the antioxidant is pentaerythritol dioctadecyl diphosphite; and the curing agent is 2-phenylimidazole.
[0036] The preparation method of the special functional phase modifier of this embodiment is:
[0037] S01: heat-treat the nano-bentonite at 300-350°C for 10-20 min, then cool to 55°C at a rate of 2-5°C / min and keep warm;
[0038] 4-7 parts of the insulated nano-bentonite are added to 8-12 parts of a phosphate buffer solution with a pH value of 5.5, and then 2-3 parts of nano-silica sol and 1-3 parts of a sodium citrate solution with a mass fraction of 4-6% are added for stirring, and then washed with water and dried to obtain a nano-bentonite conditioner;
[0039] S02: immersing the silicon carbide whisker in a yttrium nitrate solution of 4 to 7 times the total amount of the silicon carbide whisker, immersing the solution fully, with an immersion power of 350 to 400 W, immersing for 20 to 30 minutes, and completing the immersion to obtain a modified yttrium silicon carbide whisker agent;
[0040] S03: Mix 1-3 parts of silane coupling agent KH550, 2-4 parts of carboxymethyl cellulose and 2-5 parts of sodium alginate solution to obtain a compatibilizing agent;
[0041] Add the phase agent to the modified yttrium silicon carbide whisker agent in a weight ratio of 2:5 and continue to mix well to obtain a phase-adjusted silicon carbide whisker agent;
[0042] S04: The phase-adjusting silicon carbide whisker agent and nano-bentonite regulator are mixed in a weight ratio of 3:5 and ball-milled at a ball-milling speed of 1000 r / min for 1 to 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a special functional phase-adjusting agent.
[0043] The mass fraction of the sodium alginate solution in this embodiment is 4-7%; the mass fraction of the yttrium nitrate solution is 2-5%; the rotation speed of the stirring process is 550-750 r / min, and the stirring time is 35-45 min.
[0044] The preparation method of the modified nano alumina agent of this embodiment is:
[0045] S11: irradiating the nano-alumina in a proton irradiation box for 10-15 minutes at an irradiation power of 350-400W, and obtaining irradiated nano-alumina after the irradiation is completed;
[0046] The irradiated nano-alumina, sodium silicate solution and lanthanum chloride solution are mixed in a weight ratio of (2-5): (4-7): 2 to obtain a nano-alumina modified solution;
[0047] S12: The nano-alumina modified liquid and the performance-adjusting agent doped with aluminum silicate fiber are mixed in a weight ratio of (5-7):3 and ball-milled at a speed of 1500-2000 r / min for 1 hour. After the ball milling is completed, the mixture is washed with water and dried to obtain a modified nano-alumina agent.
[0048] The mass fraction of the sodium silicate solution in this embodiment is 2-5%; the mass fraction of the lanthanum chloride solution is 3-6%.
[0049] The preparation method of the performance-adjusting agent doped with aluminum silicate fiber in this embodiment is as follows:
[0050] 4-7 parts of aluminum silicate fiber and 1-3 parts of silane coupling agent KH560 are added to 5-8 parts of chitosan solution, and then 2-4 parts of hydroxyapatite and 2-3 parts of sodium dodecylbenzene sulfonate are added and blended for ultrasonic treatment at an ultrasonic power of 400-500 W for 30-40 minutes. After the ultrasonic treatment is completed, the mixture is washed with water and dried to obtain a performance-enhancing agent doped with aluminum silicate fiber.
[0051] The mass fraction of the chitosan solution in this embodiment is 2-5%.
[0052] A method for preparing a high temperature resistant fire retardant coating powder of the present embodiment comprises the following steps:
[0053] The raw materials are weighed according to weight, mixed, and then sent into a twin-screw extruder for extrusion at an extrusion temperature of 90-95°C and an extrusion speed of 450-500r / min to obtain an extrudate, which is then ground through 200 meshes to obtain a high-temperature resistant fire-retardant coating powder.
[0054] Example 1
[0055] A high temperature resistant fire retardant coating powder of this embodiment includes the following raw materials in parts by weight:
[0056] 35 parts of phenolic epoxy resin, 15 parts of bisphenol A epoxy resin with an epoxy equivalent of 1000, 10 parts of special functional phase modifier, 8 parts of curing agent, 5 parts of modified nano alumina agent, 4 parts of flame retardant, 2 parts of antioxidant, and 2 parts of dispersant.
[0057] The flame retardant of this embodiment is magnesium hydroxide; the dispersant is calcium stearate; the antioxidant is pentaerythritol dioctadecyl diphosphite; and the curing agent is 2-phenylimidazole.
[0058] The preparation method of the special functional phase modifier of this embodiment is:
[0059] S01: heat-treat the nano-bentonite at 300°C for 10 min, then cool to 55°C at a rate of 2°C / min and keep warm;
[0060] 4 parts of the insulated nano-bentonite are added to 8 parts of a phosphate buffer solution with a pH value of 5.5, and then 2 parts of nano-silica sol and 1 part of a sodium citrate solution with a mass fraction of 4-6% are added for stirring, and then washed with water and dried to obtain a nano-bentonite conditioner;
[0061] S02: immersing the silicon carbide whisker in a yttrium nitrate solution of 4 times the total amount of the silicon carbide whisker, immersing the solution fully, the immersion power is 350W, immersing for 20 minutes, and the immersion is completed to obtain a modified yttrium silicon carbide whisker agent;
[0062] S03: Mix 1 part of silane coupling agent KH550, 2 parts of carboxymethyl cellulose and 2 parts of sodium alginate solution to obtain a phase agent;
[0063] Add the phase agent to the modified yttrium silicon carbide whisker agent in a weight ratio of 2:5 and continue to mix well to obtain a phase-adjusted silicon carbide whisker agent;
[0064] S04: The phase-adjusting silicon carbide whisker agent and nano-bentonite regulator are mixed in a weight ratio of 3:5 and ball-milled at a ball-milling speed of 1000 r / min for 1 hour. After the ball-milling is completed, the mixture is washed with water and dried to obtain a special functional phase-adjusting agent.
[0065] The mass fraction of the sodium alginate solution in this embodiment is 4%; the mass fraction of the yttrium nitrate solution is 2%; the rotation speed of the stirring process is 550 r / min, and the stirring time is 35 min.
[0066] The preparation method of the modified nano alumina agent of this embodiment is:
[0067] S11: irradiating the nano-alumina in a proton irradiation box for 10 minutes at an irradiation power of 350 W, and obtaining irradiated nano-alumina after the irradiation is completed;
[0068] The irradiated nano-alumina, sodium silicate solution and lanthanum chloride solution are mixed in a weight ratio of 2:4:2 to obtain a nano-alumina modified solution;
[0069] S12: The nano-alumina modified liquid and the performance-adjusting agent doped with aluminum silicate fiber are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1500 r / min for 1 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a modified nano-alumina agent.
[0070] The mass fraction of the sodium silicate solution in this embodiment is 2%; the mass fraction of the lanthanum chloride solution is 6%.
[0071] The preparation method of the performance-adjusting agent doped with aluminum silicate fiber in this embodiment is as follows:
[0072] 4 parts of aluminum silicate fiber and 1 part of silane coupling agent KH560 were added to 5 parts of chitosan solution, and then 2 parts of hydroxyapatite and 2 parts of sodium dodecylbenzene sulfonate were added and blended for ultrasonic treatment. The ultrasonic power was 400 W and the ultrasonic treatment lasted for 30 minutes. After the ultrasonic treatment was completed, the mixture was washed with water and dried to obtain a performance-enhancing agent doped with aluminum silicate fiber.
[0073] The mass fraction of the chitosan solution in this embodiment is 2%.
[0074] A method for preparing a high temperature resistant fire retardant coating powder of the present embodiment comprises the following steps:
[0075] The raw materials were weighed according to weight, mixed, and then sent to a twin-screw extruder for extrusion at an extrusion temperature of 90° C. and an extrusion speed of 450 r / min to obtain an extrudate, which was ground through 200 meshes to obtain a high-temperature resistant fire-retardant coating powder.
[0076] Example 2
[0077] A high temperature resistant fire retardant coating powder of this embodiment includes the following raw materials in parts by weight:
[0078] 45 parts of phenolic epoxy resin, 25 parts of bisphenol A epoxy resin with epoxy equivalent of 1000, 15 parts of special functional phase modifier, 12 parts of curing agent, 8 parts of modified nano alumina agent, 7 parts of flame retardant, 3 parts of antioxidant and 3 parts of dispersant.
[0079] The flame retardant of this embodiment is magnesium hydroxide; the dispersant is calcium stearate; the antioxidant is pentaerythritol dioctadecyl diphosphite; and the curing agent is 2-phenylimidazole.
[0080] The preparation method of the special functional phase modifier of this embodiment is:
[0081] S01: heat-treat the nano-bentonite at 350°C for 20 min, then cool to 55°C at a rate of 5°C / min and keep warm;
[0082] 7 parts of the insulated nano-bentonite are added to 12 parts of a phosphate buffer solution with a pH value of 5.5, and then 3 parts of nano-silica sol and 3 parts of a 6% sodium citrate solution are added and stirred, and then washed with water and dried to obtain a nano-bentonite conditioner;
[0083] S02: immersing the silicon carbide whisker in a yttrium nitrate solution with a volume of 7 times the total volume of the silicon carbide whisker, immersing the solution fully at a power of 400 W for 30 minutes, and completing the immersion to obtain a modified yttrium silicon carbide whisker agent;
[0084] S03: Mix 3 parts of silane coupling agent KH550, 4 parts of carboxymethyl cellulose and 5 parts of sodium alginate solution to obtain a phase agent;
[0085] Add the phase agent to the modified yttrium silicon carbide whisker agent in a weight ratio of 2:5 and continue to mix well to obtain a phase-adjusted silicon carbide whisker agent;
[0086] S04: The phase-adjusting silicon carbide whisker agent and nano-bentonite regulator are mixed in a weight ratio of 3:5 and ball-milled at a ball-milling speed of 1000 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a special functional phase-adjusting agent.
[0087] The mass fraction of the sodium alginate solution in this embodiment is 7%; the mass fraction of the yttrium nitrate solution is 5%; the rotation speed of the stirring process is 750 r / min, and the stirring time is 45 min.
[0088] The preparation method of the modified nano alumina agent of this embodiment is:
[0089] S11: irradiating the nano-alumina in a proton irradiation box for 15 minutes at an irradiation power of 400 W, and obtaining irradiated nano-alumina after the irradiation is completed;
[0090] The irradiated nano-alumina, sodium silicate solution and lanthanum chloride solution are mixed in a weight ratio of 5:7:2 to obtain a nano-alumina modified solution;
[0091] S12: The nano-alumina modified liquid and the performance-adjusting agent doped with aluminum silicate fiber are mixed in a weight ratio of 7:3 and ball-milled at a speed of 2000 r / min for 1 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a modified nano-alumina agent.
[0092] The mass fraction of the sodium silicate solution in this embodiment is 5%; the mass fraction of the lanthanum chloride solution is 6%.
[0093] The preparation method of the performance-adjusting agent doped with aluminum silicate fiber in this embodiment is as follows:
[0094] 7 parts of aluminum silicate fiber and 3 parts of silane coupling agent KH560 were added to 8 parts of chitosan solution, and then 4 parts of hydroxyapatite and 3 parts of sodium dodecylbenzene sulfonate were added and blended for ultrasonic treatment. The ultrasonic power was 500W and the ultrasonic treatment lasted for 40 minutes. After the ultrasonic treatment was completed, the mixture was washed with water and dried to obtain a performance-enhancing agent doped with aluminum silicate fiber.
[0095] The mass fraction of the chitosan solution in this embodiment is 5%.
[0096] A method for preparing a high temperature resistant fire retardant coating powder of the present embodiment comprises the following steps:
[0097] The raw materials were weighed according to weight, mixed, and then sent to a twin-screw extruder for extrusion at an extrusion temperature of 95° C. and an extrusion speed of 500 r / min to obtain an extrudate, which was then ground through 200 meshes to obtain a high-temperature resistant fire-retardant coating powder.
[0098] Example 3
[0099] A high temperature resistant fire retardant coating powder of this embodiment includes the following raw materials in parts by weight:
[0100] 40 parts of phenolic epoxy resin, 20 parts of bisphenol A epoxy resin with epoxy equivalent of 1000, 12.5 parts of special functional phase modifier, 10 parts of curing agent, 6.5 parts of modified nano alumina agent, 5.5 parts of flame retardant, 2.5 parts of antioxidant and 2.5 parts of dispersant.
[0101] The flame retardant of this embodiment is magnesium hydroxide; the dispersant is calcium stearate; the antioxidant is pentaerythritol dioctadecyl diphosphite; and the curing agent is 2-phenylimidazole.
[0102] The preparation method of the special functional phase modifier of this embodiment is:
[0103] S01: heat-treat the nano-bentonite at 325°C for 15 min, then cool to 55°C at a rate of 3.5°C / min and keep warm;
[0104] 5.5 parts of the insulated nano-bentonite are added to 10 parts of a phosphate buffer solution with a pH value of 5.5, and then 2.5 parts of nano-silica sol and 2 parts of a 5% by mass sodium citrate solution are added and stirred, and then washed with water and dried to obtain a nano-bentonite conditioner;
[0105] S02: immersing the silicon carbide whisker in a yttrium nitrate solution with a volume of 5.5 times the total volume of the silicon carbide whisker, immersing the solution fully at a power of 375 W for 25 minutes, and completing the immersion to obtain a modified yttrium silicon carbide whisker agent;
[0106] S03: 2 parts of silane coupling agent KH550, 3 parts of carboxymethyl cellulose and 3.5 parts of sodium alginate solution are mixed to obtain a phase agent;
[0107] Add the phase agent to the modified yttrium silicon carbide whisker agent in a weight ratio of 2:5 and continue to mix well to obtain a phase-adjusted silicon carbide whisker agent;
[0108] S04: The phase-adjusting silicon carbide whisker agent and nano-bentonite regulator are mixed in a weight ratio of 3:5 and ball-milled at a ball-milling speed of 1000 r / min for 1.5 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a special functional phase-adjusting agent.
[0109] The mass fraction of the sodium alginate solution in this embodiment is 5.5%; the mass fraction of the yttrium nitrate solution is 3.5%; the rotation speed of the stirring process is 600 r / min, and the stirring time is 40 min.
[0110] The preparation method of the modified nano alumina agent of this embodiment is:
[0111] S11: irradiating the nano-alumina in a proton irradiation box for 12.5 minutes at an irradiation power of 375 W, and obtaining irradiated nano-alumina after the irradiation is completed;
[0112] The irradiated nano-alumina, sodium silicate solution and lanthanum chloride solution are mixed in a weight ratio of 3.5:5.5:2 to obtain a nano-alumina modified solution;
[0113] S12: Mix the nano-alumina modified liquid and the performance-adjusting agent doped with aluminum silicate fiber in a weight ratio of 2:1, and perform ball milling at a ball milling speed of 1750 r / min for 1 h. After the ball milling is completed, wash with water, and dry to obtain a modified nano-alumina agent.
[0114] The mass fraction of the sodium silicate solution in this embodiment is 3.5%; the mass fraction of the lanthanum chloride solution is 4.5%.
[0115] The preparation method of the performance-adjusting agent doped with aluminum silicate fiber in this embodiment is as follows:
[0116] 5.5 parts of aluminum silicate fiber and 2 parts of silane coupling agent KH560 were added to 6.5 parts of chitosan solution, and then 3 parts of hydroxyapatite and 2.5 parts of sodium dodecylbenzene sulfonate were added and blended for ultrasonic treatment. The ultrasonic power was 450W and the ultrasonic treatment lasted for 35 minutes. After the ultrasonic treatment was completed, the mixture was washed with water and dried to obtain a performance-enhancing agent doped with aluminum silicate fiber.
[0117] The mass fraction of the chitosan solution in this embodiment is 3.5%.
[0118] A method for preparing a high temperature resistant fire retardant coating powder of the present embodiment comprises the following steps:
[0119] The raw materials were weighed according to weight, mixed, and then sent to a twin-screw extruder for extrusion at an extrusion temperature of 92.5° C. and an extrusion speed of 470 r / min to obtain an extrudate, which was ground through 200 meshes to obtain a high-temperature resistant fire-retardant coating powder.
[0120] The flame retardant properties of Examples 1-3 were tested, and the test results were as follows:
[0121]
[0122] The test results in Examples 1-3 show that the products of Examples 1-3 of the present invention have excellent flame retardant properties and significant flame retardant effects.
[0123] Comparative Example 1
[0124] The difference from Example 3 is that no special functional phase adjusting agent is added.
[0125] Comparative Example 2
[0126] The difference from Example 3 is that no nano bentonite regulator is added in the preparation of the special functional phase modifier.
[0127] Comparative Example 3
[0128] The difference from Example 3 is that nano bentonite raw material is directly used as a substitute in the preparation of the nano bentonite regulator.
[0129] Comparative Example 4
[0130] The difference from Example 3 is that no phase-adjusting silicon carbide whisker agent is added in the preparation of the special functional phase-adjusting agent.
[0131] Comparative Example 5
[0132] The difference from Example 3 is that no phase agent is added in the preparation of the phase-adjusting silicon carbide whisker agent.
[0133] Comparative Example 6
[0134] The difference from Example 3 is that no modified yttrium silicon carbide whisker is added in the preparation of the phase-adjusted silicon carbide whisker.
[0135] Comparative Example 7
[0136] The difference from Example 3 is that the yttrium-modified silicon carbide whisker agent is directly replaced by silicon carbide whiskers.
[0137] Comparative Example 8
[0138] The difference from Example 3 is that no performance-enhancing agent for doping aluminum silicate fibers is added.
[0139] Comparative Example 9
[0140] The difference from Example 3 is that the preparation method of the nano-alumina modified liquid in the preparation of the performance-adjusting agent doped with aluminum silicate fiber is different: the nano-alumina and lanthanum chloride solution are mixed in a weight ratio of 2:5 to obtain the nano-alumina modified liquid.
[0141] Comparative Example 10
[0142] The difference from Example 3 is that the conditioning agent doped with aluminum silicate fibers is not used in the preparation of the conditioning agent doped with aluminum silicate fibers.
[0143] The products of Examples 1 to 3 and Comparative Examples 1 to 10 were sprayed onto a substrate using an electrostatic spraying technique with a spraying thickness of 1.0 mm, and then tested for high temperature resistance, adhesion (GB / T5210 standard test) and wear resistance (GB / T1768-2006 test standard); and the products were irradiated at 50 mw / m and UV intensity for 6 h, and then placed under 2% hydrochloric acid mist conditions for 12 h. The above treatment was one cycle, and a total of 10 cycles were processed to test the acid resistance and UV resistance stability of the products; the test results are as follows:
[0144]
[0145] It can be seen from Comparative Examples 1 to 10 and Examples 1 to 3 that:
[0146] The product of Example 3 has excellent high temperature resistance, and also excellent adhesion and wear resistance, and the three can be improved in a coordinated manner. In addition, the product has significant stability under acid and UV resistance conditions;
[0147] From comparative examples 1 to 10 and embodiment 3, it can be seen that the performance of the product is significantly deteriorated when no special functional phase modifier and no performance modifier doped with aluminum silicate fiber are added in the present invention. The performance effect of the product is most obvious when the two are coordinated and work together.
[0148] The performance of the products tends to deteriorate when no nano-bentonite regulator is added in the preparation of special functional phase modifiers, nano-bentonite raw materials are used directly to replace nano-bentonite regulators, silicon carbide whiskers for phase modulation are not added in the preparation of special functional phase modifiers, phase modifiers are not added in the preparation of silicon carbide whiskers for phase modulation, yttrium-modified silicon carbide whiskers are not added in the preparation of silicon carbide whiskers for phase modulation, and silicon carbide whiskers are used directly to replace yttrium-modified silicon carbide whiskers.
[0149] The phase-adjusted silicon carbide whisker agent obtained by mixing the modified yttrium silicon carbide whisker agent obtained by the method of the present invention with the phase agent is the most significant product performance effect obtained by combining with the nano-bentonite regulator of the present invention, and other methods are not as obvious as the effect of the present invention;
[0150] The performance of the products tends to deteriorate when the preparation method of the nano-alumina modified liquid is different in the preparation of the performance-enhancing agent doped with aluminum silicate fiber and the performance-enhancing agent doped with aluminum silicate fiber is not used. In addition, the performance of the products deteriorates more obviously when the performance-enhancing agent doped with aluminum silicate fiber is not used.
[0151] The present invention further explores the product performance by preparing an efficiency regulator doped with aluminum silicate fiber;
[0152] The preparation method of the performance-adjusting agent doped with aluminum silicate fiber is as follows:
[0153] 5.5 parts of aluminum silicate fiber and 2 parts of silane coupling agent KH560 were added to 6.5 parts of chitosan solution, and then 3 parts of hydroxyapatite and 2.5 parts of sodium dodecylbenzene sulfonate were added and blended for ultrasonic treatment. The ultrasonic power was 450W and the ultrasonic treatment lasted for 35 minutes. After the ultrasonic treatment was completed, the mixture was washed with water and dried to obtain a performance-enhancing agent doped with aluminum silicate fiber.
[0154] Experimental Example 1
[0155] The only difference from Example 3 is that aluminum silicate fibers are not added in the preparation of the performance-enhancing agent doped with aluminum silicate fibers.
[0156] Experimental Example 2
[0157] The only difference from Example 3 is that the silane coupling agent KH560 and sodium dodecylbenzene sulfonate are not added in the preparation of the conditioning agent doped with aluminum silicate fiber.
[0158] Experimental Example 3
[0159] The only difference from Example 3 is that deionized water is used instead of chitosan solution in the preparation of the conditioning agent doped with aluminum silicate fiber.
[0160] Experimental Example 4
[0161] The only difference from Example 3 is that hydroxyapatite is not added in the preparation of the conditioning agent doped with aluminum silicate fibers.
[0162] The test results of Experimental Examples 1-4 are as follows:
[0163]
[0164] It can be seen from Experimental Examples 1-4 that aluminum silicate fiber is not added in the preparation of the performance-enhancing agent doped with aluminum silicate fiber, and the performance changes of the product are most obvious in the performance-enhancing agent doped with aluminum silicate fiber, followed by the fact that hydroxyapatite is not added. The product performance effect is significantly improved by the formulation of hydroxyapatite and aluminum silicate fiber. At the same time, silane coupling agent KH560 and sodium dodecylbenzene sulfonate are not added in the preparation of the performance-enhancing agent doped with aluminum silicate fiber, and deionized water is used instead of chitosan solution. The performance of the product has a tendency to deteriorate to varying degrees. Only the performance-enhancing agent doped with aluminum silicate fiber obtained by the specific method of the present invention has the most significant product performance effect, and the effects of other methods are not as obvious as those of the present invention.
[0165] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0166] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A high temperature resistant fire retardant coating powder, characterized in that: It includes the following raw materials in parts by weight: 35-45 parts of phenolic epoxy resin, 15-25 parts of bisphenol A epoxy resin with an epoxy equivalent of 1000, 10-15 parts of special functional phase modifier, 8-12 parts of curing agent, 5-8 parts of modified nano alumina agent, 4-7 parts of flame retardant, 2-3 parts of antioxidant and 2-3 parts of dispersant; Wherein, the preparation method of the special functional phase modifier is: S01: heat-treat the nano-bentonite at 300-350°C for 10-20 min, then cool to 55°C at a rate of 2-5°C / min and keep warm; 4-7 parts of the insulated nano-bentonite are added to 8-12 parts of a phosphate buffer solution with a pH value of 5.5, and then 2-3 parts of nano-silica sol and 1-3 parts of a sodium citrate solution with a mass fraction of 4-6% are added for stirring, and then washed with water and dried to obtain a nano-bentonite conditioner; S02: immersing the silicon carbide whisker in a yttrium nitrate solution of 4 to 7 times the total amount of the silicon carbide whisker, immersing the solution fully, with an immersion power of 350 to 400 W, immersing for 20 to 30 minutes, and completing the immersion to obtain a modified yttrium silicon carbide whisker agent; S03: Mix 1-3 parts of silane coupling agent KH550, 2-4 parts of carboxymethyl cellulose and 2-5 parts of sodium alginate solution to obtain a compatibilizing agent; Add the phase agent to the modified yttrium silicon carbide whisker agent in a weight ratio of 2:5 and continue to mix well to obtain a phase-adjusted silicon carbide whisker agent; S04: mixing the phase-adjusting silicon carbide whisker agent and the nano-bentonite regulator in a weight ratio of 3:5, and subjecting the mixture to ball milling. The ball milling speed is 1000 r / min, and the ball milling is performed for 1 to 2 hours. After the ball milling is completed, the mixture is washed with water and dried to obtain a special functional phase-adjusting agent. Wherein, the preparation method of the modified nano alumina agent is: S11: irradiating the nano-alumina in a proton irradiation box for 10-15 minutes at an irradiation power of 350-400W, and obtaining irradiated nano-alumina after the irradiation is completed; The irradiated nano-alumina, sodium silicate solution and lanthanum chloride solution are mixed in a weight ratio of (2-5): (4-7): 2 to obtain a nano-alumina modified solution; S12: mixing the nano-alumina modified liquid and the performance-adjusting agent doped with aluminum silicate fiber in a weight ratio of (5-7):3, and ball milling the mixture at a speed of 1500-2000 r / min for 1 h. After the ball milling is completed, washing with water and drying are performed to obtain a modified nano-alumina agent. Wherein, the preparation method of the performance-adjusting agent doped with aluminum silicate fiber is: 4-7 parts of aluminum silicate fiber and 1-3 parts of silane coupling agent KH560 are added to 5-8 parts of chitosan solution, and then 2-4 parts of hydroxyapatite and 2-3 parts of sodium dodecylbenzene sulfonate are added and blended for ultrasonic treatment at an ultrasonic power of 400-500 W for 30-40 minutes. After the ultrasonic treatment is completed, the mixture is washed with water and dried to obtain a performance-enhancing agent doped with aluminum silicate fiber.
2. A high temperature resistant fire retardant coating powder according to claim 1, characterized in that: The high temperature resistant fire retardant coating powder comprises the following raw materials in parts by weight: 40 parts of phenolic epoxy resin, 20 parts of bisphenol A epoxy resin with epoxy equivalent of 1000, 12.5 parts of special functional phase modifier, 10 parts of curing agent, 6.5 parts of modified nano alumina agent, 5.5 parts of flame retardant, 2.5 parts of antioxidant and 2.5 parts of dispersant.
3. The high temperature resistant fire retardant coating powder according to claim 1, characterized in that: The flame retardant is magnesium hydroxide; the dispersant is calcium stearate; the antioxidant is pentaerythritol dioctadecyl diphosphite; and the curing agent is 2-phenylimidazole.
4. The high temperature resistant fire retardant coating powder according to claim 1, characterized in that: The mass fraction of the sodium alginate solution is 4-7%; the mass fraction of the yttrium nitrate solution is 2-5%; The stirring speed is 550~750r / min, and the stirring time is 35~45min.
5. The high temperature resistant fire retardant coating powder according to claim 1, characterized in that: The mass fraction of the sodium silicate solution is 2-5%; the mass fraction of the lanthanum chloride solution is 3-6%.
6. The high temperature resistant fire retardant coating powder according to claim 1, characterized in that: The mass fraction of the chitosan solution is 2-5%.
7. A method for preparing a high temperature resistant fire retardant coating powder according to any one of claims 1 to 6, characterized in that: The following steps are involved: The raw materials are weighed according to weight, mixed, and then sent into a twin-screw extruder for extrusion at an extrusion temperature of 90-95°C and an extrusion speed of 450-500r / min to obtain an extrudate, which is then ground through 200 meshes to obtain a high-temperature resistant fire-retardant coating powder.
Citation Information
Patent Citations
Flame-retardant material for interior trim parts of automobiles and preparation method of flame-retardant material
CN117924875A
High-temperature-resistant heat-conducting insulating paint and preparation method thereof
CN117925055A