A kind of water-based multifunctional coating and preparation method thereof
Modified chitosan by functionalizing ZnO/Fe3O4 polyaniline in thiourea improves acid resistance and alkali resistance in water-based coatings, solves the corrosion problem of water-based coatings in high-salt environments, and achieves better corrosion resistance and Low cost production.
Patent Information
- Application Number
- CN202411260566.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-10
AI Technical Summary
In the prior art, PANI/CTS composite materials are rarely used as corrosion inhibitors for water-based coatings, resulting in insufficient corrosion resistance of water-based coatings in acid resistance, alkali resistance and high salt environments.
Using thiourea functionalized ZnO/Fe3O4 polyaniline to modify chitosan, add modified chitosan, antibacterial agent, leveling agent, aqueous dispersant and aqueous defoaming agent to the aqueous polyurethane to form a water-based multifunctional coating, which improves the The coatings are acid and alkali resistant and maintain corrosion resistance in high salt environments.
It significantly improves the acid resistance and alkali resistance of water-based coatings, enhances corrosion resistance in high-salt environments, is low in cost and simple in preparation, and is suitable for market promotion.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based coatings, and in particular to a water-based multifunctional coating and a preparation method thereof. Background Art
[0002] The main function of anti-corrosion coatings is to form a protective film on the surface of metals or other materials, effectively isolating external corrosive media such as moisture, oxygen, chemicals, etc., thereby preventing the material from corroding. This coating not only has a shielding effect, reducing the contact between the corrosive medium and the material, but may also contain corrosion-inhibiting pigments, which neutralize acidic substances or generate metal soaps through chemical reactions to enhance the corrosion resistance of the material. In addition, some anti-corrosion coatings use highly active metals such as zinc powder through electrochemical action to form micro-batteries between the coating and the substrate, protecting the substrate from corrosion in the form of sacrificial anodes. Therefore, anti-corrosion coatings are an important means to extend the service life of materials and reduce maintenance costs.
[0003] As a natural material, chitosan has attracted increasing attention due to its excellent biocompatibility, biodegradability, good adhesion and non-toxic properties. Chitosan contains electron-rich hydroxyl and amino groups, and the lone pairs of electrons in these groups can form strong coordination bonds with metal surfaces, enabling them to function as corrosion inhibitors.
[0004] Polyaniline (PANI) is a conductive polymer that has been used as a promising environmentally friendly corrosion inhibitor. It is easy to prepare at low cost, exhibits good electrical conductivity and low toxicity, and has a fully reversible redox cycle.
[0005] There are few reports in the prior art on the application of PANI / CTS composites as corrosion inhibitors in water-based coatings. Summary of the invention
[0006] In order to solve the problems existing in the prior art, the present invention provides a water-based multifunctional coating and a preparation method thereof.
[0007] The present invention is achieved through the following technical solutions:
[0008] A water-based multifunctional coating is composed of the following raw materials in parts by weight: 40 parts of water-based polyurethane, 0.5-3 parts of thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan, 0.3 parts of an antibacterial agent, 0.8 parts of a leveling agent, 1 part of a water-based dispersant, 0.8 parts of a water-based defoaming agent, and 25 parts of deionized water.
[0009] Furthermore, the main component of the antibacterial agent is benzisothiazolinone.
[0010] Furthermore, the leveling agent is BASF EFKA-3033; the aqueous dispersant is BASF CX 4320AM; and the aqueous defoaming agent is BASF Efka FA 2620 AN.
[0011] Nano-ZnO can promote the formation of Zn3(PO4)2·4H2O and Zn2Fe(PO4)2·4H2O in the coating and improve the corrosion resistance, but unmodified nano-ZnO is insoluble in water and needs to be modified.
[0012] Furthermore, the preparation method of the thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan is:
[0013] ZnO nanoparticles were added to the thiourea aqueous solution and stirred at room temperature for 30 min. The precipitate was washed several times with distilled water and then dried at 80 °C for 3 h to obtain thiourea functionalized ZnO.
[0014] Polyaniline-modified chitosan was added to acetic acid water, stirred for 5 h, and then ultrasonicated for 1 h; then thiourea-functionalized ZnO was added, stirred for 3 h, and then Fe3O4 nanoparticles were added, and 0.1 mol / L NaOH was slowly added and stirred to adjust the pH until the pH was 7; the solution was filtered, washed with distilled water several times, and the precipitate was vacuum dried at 60°C for 12 h to obtain thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan.
[0015] Furthermore, the average particle size of the ZnO nanoparticles is 40 nm; the average particle size of the Fe3O4 nanoparticles is 50 nm.
[0016] Furthermore, the preparation method of the polyaniline modified chitosan is:
[0017] Dissolve chitosan in acetic acid water, add polyaniline monomer and stir at room temperature for 0.5h;
[0018] Then, ammonium persulfate was added dropwise at 0-5°C; the solution was stirred at 0-5°C for 6 hours, centrifuged to obtain a precipitate, washed with distilled water for 5 times, and then the precipitate was vacuum dried at 60°C for 12 hours to obtain polyaniline / modified chitosan.
[0019] Furthermore, a method for preparing a water-based multifunctional coating is provided, comprising the following steps: mixing water-based polyurethane with deionized water and stirring for 5 minutes, then adding modified chitosan, ultrasonically mixing the solution for 10 minutes, then adding an antibacterial agent, a leveling agent, a water-based dispersant, and a water-based defoaming agent, and stirring for 0.5 hours to obtain a water-based multifunctional coating.
[0020] Compared with the prior art, the present invention has the following advantages and beneficial effects: by using polyaniline to modify chitosan, and further inserting ZnO / Fe3O4 nanomaterials into the polyaniline-modified chitosan, the acid resistance and alkali resistance of the water-based coating are improved, and ZnO is further modified to improve the acid resistance in a high-salt environment. The original preparation is simple, the cost is low, and it is conducive to market promotion. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The illustrative embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0022] In the present invention, Fe3O4 nanoparticles were purchased from Sigma-Aldrich, with an average particle size of 50nm, no surface modification, a concentration of 1mg / mL, and a solvent of water, and were used after vacuum drying; ZnO nanoparticles were purchased from Sigma-Aldrich, with an average particle size of 40nm, a concentration of 20wt%, dissolved in water, a density of 1.7g / mL, and were used after vacuum drying. The antibacterial agent was purchased from Shandong Kasong New Materials Company, model BIT20, the main component of which was benzisothiazolinone; the leveling agent was BASF EFKA-3033; the water-based dispersant was BASF CX 4320AM; the water-based defoamer was BASF Efka FA 2620 AN, and the remaining reagents were all commercially available products.
[0023] Example 1: A water-based multifunctional coating is composed of the following raw materials in parts by weight: 40 parts of water-based polyurethane, 0.5 parts of thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan, 0.3 parts of an antibacterial agent, 0.8 parts of a leveling agent, 1 part of a water-based dispersant, 0.8 parts of a water-based defoaming agent, and 25 parts of deionized water.
[0024] A preparation method of a water-based multifunctional coating comprises: mixing water-based polyurethane with deionized water and stirring for 5 minutes, then adding thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan, ultrasonically mixing the solution for 10 minutes, then adding an antibacterial agent, a leveling agent, a water-based dispersant, and a water-based defoaming agent, stirring for 0.5 hours, and obtaining a water-based multifunctional coating.
[0025] The preparation of thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan:
[0026] 1.2 g ZnO nanoparticles were added to 25 mL 1 M thiourea aqueous solution and stirred at room temperature for 30 min. The precipitate was washed several times with distilled water and then dried at 80 °C for 3 h to obtain thiourea functionalized ZnO.
[0027] Take 2.5g polyaniline-modified chitosan and add it to 150 mL 1% v / v acetic acid water, stir for 5h, and then ultrasonicate for 1h; then add 0.3g thiourea-functionalized ZnO, stir for 3h, and then add 0.3g Fe3O4 nanoparticles, slowly add 0.1mol / L NaOH and stir to adjust the pH until the pH is 7; filter the solution, wash with distilled water several times, and vacuum dry the precipitate at 60°C for 12h to obtain thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan.
[0028] Preparation of polyaniline modified chitosan:
[0029] Take 2 g of chitosan and dissolve it in 200 mL of 0.33 M acetic acid water, add 24 mmol of polyaniline monomer and stir at room temperature for 0.5 h, wherein the polyaniline monomer is dissolved in 40 mL of 0.8 M NH2SO3H aqueous solution;
[0030] Then, 10 mmol of ammonium persulfate was added dropwise at 0-5°C, wherein the ammonium persulfate was dissolved in a 0.33 acetic acid aqueous solution; the solution was stirred at 0-5°C for 6 hours, centrifuged to obtain a precipitate, washed with distilled water for 5 times, and then vacuum dried at 60°C for 12 hours to obtain polyaniline / modified chitosan.
[0031] Example 2: A water-based multifunctional coating is composed of the following raw materials in parts by weight: 40 parts of water-based polyurethane, 1 part of thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan, 0.3 parts of an antibacterial agent, 0.8 parts of a leveling agent, 1 part of an aqueous dispersant, 0.8 parts of an aqueous defoaming agent, and 25 parts of deionized water.
[0032] A preparation method of a water-based multifunctional coating comprises: mixing water-based polyurethane with deionized water and stirring for 5 minutes, then adding thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan, ultrasonically mixing the solution for 10 minutes, then adding an antibacterial agent, a leveling agent, a water-based dispersant, and a water-based defoaming agent, stirring for 0.5 hours, and obtaining a water-based multifunctional coating.
[0033] The preparation method of thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan is the same as that in Example 1.
[0034] Example 3: A water-based multifunctional coating is composed of the following raw materials in parts by weight: 40 parts of water-based polyurethane, 2 parts of thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan, 0.3 parts of an antibacterial agent, 0.8 parts of a leveling agent, 1 part of a water-based dispersant, 0.8 parts of a water-based defoaming agent, and 25 parts of deionized water.
[0035] A preparation method of a water-based multifunctional coating comprises: mixing water-based polyurethane with deionized water and stirring for 5 minutes, then adding thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan, ultrasonically mixing the solution for 10 minutes, then adding an antibacterial agent, a leveling agent, a water-based dispersant, and a water-based defoaming agent, stirring for 0.5 hours, and obtaining a water-based multifunctional coating.
[0036] The preparation method of thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan is the same as that in Example 1.
[0037] Example 4: A water-based multifunctional coating is composed of the following raw materials in parts by weight: 40 parts of water-based polyurethane, 2.5 parts of thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan, 0.3 parts of an antibacterial agent, 0.8 parts of a leveling agent, 1 part of a water-based dispersant, 0.8 parts of a water-based defoaming agent, and 25 parts of deionized water.
[0038] A preparation method of a water-based multifunctional coating comprises: mixing water-based polyurethane with deionized water and stirring for 5 minutes, then adding thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan, ultrasonically mixing the solution for 10 minutes, then adding an antibacterial agent, a leveling agent, a water-based dispersant, and a water-based defoaming agent, stirring for 0.5 hours, and obtaining a water-based multifunctional coating.
[0039] The preparation method of thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan is the same as that in Example 1.
[0040] Example 5: A water-based multifunctional coating is composed of the following raw materials in parts by weight: 40 parts of water-based polyurethane, 3 parts of thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan, 0.3 parts of an antibacterial agent, 0.8 parts of a leveling agent, 1 part of a water-based dispersant, 0.8 parts of a water-based defoaming agent, and 25 parts of deionized water.
[0041] A preparation method of a water-based multifunctional coating comprises: mixing water-based polyurethane with deionized water and stirring for 5 minutes, then adding thiourea-functionalized ZnO / Fe3O4 polyaniline-modified chitosan, ultrasonically mixing the solution for 10 minutes, then adding an antibacterial agent, a leveling agent, a water-based dispersant, and a water-based defoaming agent, stirring for 0.5 hours, and obtaining a water-based multifunctional coating.
[0042] The preparation method of thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan is the same as that in Example 1.
[0043] Comparative Example 1: A water-based multifunctional coating is composed of the following raw materials in parts by weight: 40 parts of water-based polyurethane, 2 parts of ZnO / Fe3O4 polyaniline-modified chitosan, 0.3 parts of antibacterial agent, 0.8 parts of leveling agent, 1 part of water-based dispersant, 0.8 parts of water-based defoaming agent, and 25 parts of deionized water.
[0044] A method for preparing a water-based multifunctional coating comprises: mixing water-based polyurethane with deionized water and stirring for 5 minutes, then adding ZnO / Fe3O4 polyaniline modified chitosan, ultrasonically mixing the solution for 10 minutes, then adding an antibacterial agent, a leveling agent, a water-based dispersant, and a water-based defoaming agent, stirring for 0.5 hours, and obtaining a water-based multifunctional coating.
[0045] The preparation of ZnO / Fe3O4 polyaniline modified chitosan:
[0046] Take 2.5g polyaniline-modified chitosan and add it to 150 mL 1% v / v acetic acid water, stir for 5h, and then ultrasonicate for 1h; then add 0.3g ZnO nanoparticles, stir for 3h, and then add 0.3g Fe3O4 nanoparticles, slowly add 0.1mol / L NaOH and stir to adjust the pH until the pH is 7; filter the solution, wash with distilled water several times, and vacuum dry the precipitate at 60°C for 12h to obtain ZnO / Fe3O4 polyaniline-modified chitosan.
[0047] Comparative Example 2: A water-based multifunctional coating is composed of the following raw materials in parts by weight: 40 parts of water-based polyurethane, 2 parts of polyaniline-modified chitosan, 0.3 parts of antibacterial agent, 0.8 parts of leveling agent, 1 part of water-based dispersant, 0.8 parts of water-based defoaming agent, and 25 parts of deionized water.
[0048] A method for preparing a water-based multifunctional coating comprises: mixing water-based polyurethane with deionized water and stirring for 5 minutes, then adding polyaniline-modified chitosan, ultrasonically mixing the solution for 10 minutes, then adding an antibacterial agent, a leveling agent, a water-based dispersant, and a water-based defoaming agent, stirring for 0.5 hours, and obtaining a water-based multifunctional coating.
[0049] The preparation of polyaniline modified chitosan:
[0050] Take 2 g of chitosan and dissolve it in 200 mL of 0.33 M acetic acid water, add 24 mmol of polyaniline monomer and stir at room temperature for 0.5 h, wherein the polyaniline monomer is dissolved in 40 mL of 0.8 M NH2SO3H aqueous solution;
[0051] Then, 10 mmol of ammonium persulfate was added dropwise at 0-5°C, wherein the ammonium persulfate was dissolved in a 0.33 acetic acid aqueous solution; the solution was stirred at 0-5°C for 6 hours, centrifuged to obtain a precipitate, washed with distilled water for 5 times, and then vacuum dried at 60°C for 12 hours to obtain polyaniline / modified chitosan.
[0052] Test Example 1: Acid resistance and alkali resistance tests were carried out in accordance with GB / T9274-1988.
[0053] Table 1 Acid and alkali resistance test
[0054]
[0055] Test Example 2: The test was conducted in a common high-salt environment. Specifically, the sample was prepared according to GB / T9274-1988, and then immersed in a 10% H2SO4 solution prepared with a mixed saturated solution of barium sulfate, strontium sulfate, calcium sulfate, and calcium carbonate to observe the performance of the paint film.
[0056] Table 2 Acid and alkali resistance test under high salt environment
[0057]
[0058] It can be seen from Table 1 and Table 2 that the chitosan modified with thiourea functionalized ZnO / Fe3O4 polyaniline, ZnO / Fe3O4 polyaniline and polyaniline modified chitosan all have a certain anti-corrosion effect, among which the thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan has no bubbles in the paint film after being immersed in 10% NaOH for 720h, and there is no bubble in 10% HC. At the same time, in a high-salt environment, the thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan also has a better acid resistance effect than the ZnO / Fe3O4 polyaniline modified chitosan and polyaniline modified chitosan.
Claims
1. A water-based multifunctional coating, characterized in that: The method is composed of the following raw materials in parts by weight: 40 parts of waterborne polyurethane, 0.5-3 parts of thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan, 0.3 parts of antibacterial agent, 0.8 parts of leveling agent, 1 part of waterborne dispersant, 0.8 parts of waterborne defoaming agent, and 25 parts of deionized water; The main component of the antibacterial agent is benzisothiazolinone; The preparation method of the thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan is as follows: ZnO nanoparticles were added to the thiourea aqueous solution and stirred at room temperature for 30 min. The precipitate was washed several times with distilled water and then dried at 80 °C for 3 h to obtain thiourea functionalized ZnO. Polyaniline-modified chitosan was added to acetic acid water, stirred for 5 h, and then ultrasonicated for 1 h. Then, thiourea-functionalized ZnO was added, stirred for 3 h, and then Fe3O4 nanoparticles were added. 0.1 mol / L NaOH was slowly added and stirred to adjust the pH until the pH was 7. The solution was filtered, washed with distilled water several times, and the precipitate was dried under vacuum at 60 °C for 12 h to obtain thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan.
2. A water-based multifunctional coating as claimed in claim 1, characterized in that: The average particle size of the ZnO nanoparticles is 40 nm; the average particle size of the Fe3O4 nanoparticles is 50 nm.
3. A water-based multifunctional coating as claimed in claim 2, characterized in that: The preparation method of the polyaniline modified chitosan is: Dissolve chitosan in acetic acid water, add polyaniline monomer and stir at room temperature for 0.5h; Then, ammonium persulfate was added dropwise at 0-5°C; the solution was stirred at 0-5°C for 6 hours, centrifuged to obtain a precipitate, washed with distilled water for 5 times, and then the precipitate was vacuum dried at 60°C for 12 hours to obtain polyaniline-modified chitosan.
4. The method for preparing a water-based multifunctional coating according to any one of claims 1 to 3, characterized in that: The following steps are involved: The waterborne polyurethane was mixed with deionized water and stirred for 5 minutes, and then thiourea functionalized ZnO / Fe3O4 polyaniline modified chitosan was added, and the solution was ultrasonically mixed for 10 minutes. Then, an antibacterial agent, a leveling agent, a water-based dispersant, and a water-based defoaming agent were added and stirred for 0.5 hours to obtain a water-based multifunctional coating.
Citation Information
Patent Citations
Environmentally-friendly anticorrosive composite coating
CN109161340A
Water-based anti-corrosion coating
CN114702866A