Backwater all-purpose adhesive with waterproof performance and preparation method thereof
By using a combination of silicate, calcium hydroxide, cement and other materials and a spray and water preparation method, the problem of aging and degradation of water-backed universal adhesive in a high-humidity environment has been solved, and its excellent waterproof performance and high performance in a humid environment have been achieved. Durability, meeting the long-term waterproofing needs of buildings.
Patent Information
- Application Number
- CN202410940796.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-15
AI Technical Summary
Existing water-backed universal adhesives are prone to aging and degradation in high-humidity and harsh environments, resulting in a decline in waterproofing performance, affecting the service life of the building and possibly causing safety hazards.
Using a combination of materials such as silicate, calcium hydroxide, cement, carboxymethylcellulose, calcium stearate, ethoxysilane, diisocyanate, nano-zinc oxide, etc., through a preparation method of spraying water and stirring evenly to form a Water-backed universal glue with excellent waterproof properties.
The weather resistance, durability and environmental protection of the water-backed universal adhesive are improved, so that it can maintain good bonding performance in humid or underwater environments, extend the service life, and be easy to operate during the construction process, improving construction efficiency and quality. .
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to a water-resistant all-purpose adhesive and a preparation method thereof. Background Art
[0002] Backwater all-purpose adhesive is a special adhesive used for waterproofing the backwater surface of building structures. It has excellent bonding strength and waterproof performance. It is widely used in waterproofing projects in humid environments such as basements, bathrooms, and pools, and is of great significance for improving the waterproof effect and service life of buildings.
[0003] At present, the widely used backwater multipurpose adhesive on the market is mainly made of organic polymer materials. This material performs well in terms of bonding strength and waterproof performance, providing reliable protection for many construction projects. However, with the continuous improvement of material performance requirements, its limitations in practical applications have gradually emerged. For example, backwater multipurpose adhesive is prone to aging and degradation in harsh environments such as high humidity. This is mainly because organic polymer materials are easy to absorb moisture in a humid environment, causing changes in the internal structure of the material, thereby affecting its waterproof performance. This performance degradation not only shortens the service life of the building, but may also cause a series of safety hazards.
[0004] Therefore, the purpose of the present invention is to provide a waterproof back water all-purpose adhesive and a preparation method thereof, aiming to solve the problems existing in the prior art and improve the weather resistance, durability and environmental protection of the back water all-purpose adhesive. Summary of the invention
[0005] In view of this, the present invention proposes a water-resistant all-purpose adhesive and a preparation method thereof, aiming to solve the problems in the current technology.
[0006] The present invention provides a water-proof multipurpose adhesive, which comprises the following components in parts by weight:
[0007] 20-30 parts of silicate, 10-20 parts of calcium hydroxide, 30-40 parts of cement, 2-5 parts of carboxymethyl cellulose, 1-3 parts of calcium stearate, 5-10 parts of waterproofing agent, 2-5 parts of cross-linking agent, 5-10 parts of silicon dioxide, 5-10 parts of silica fume, 1-3 parts of nano zinc oxide and 18-24 parts of water.
[0008] Preferably, the particle size of the silicon dioxide is 60-100 mesh.
[0009] Preferably, the waterproofing agent is ethoxysilane;
[0010] And / or, the cross-linking agent is diisocyanate.
[0011] Preferably, the preparation method of the carboxymethyl cellulose comprises:
[0012] The lignocellulose is dissolved in a mixed solution of sodium hydroxide and chloroacetic acid to react to obtain sodium carboxymethyl cellulose, which is then acidified with hydrochloric acid, washed and dried to obtain the carboxymethyl cellulose.
[0013] Preferably, the preparation method of the nano zinc oxide comprises:
[0014] The zinc salt solution is reacted with an alkaline solution to generate zinc hydroxide precipitate, which is then pyrolyzed at 300-600°C to obtain zinc oxide particles;
[0015] The zinc oxide particles are calcined at 400-800° C. and then cooled to obtain the nano zinc oxide.
[0016] Preferably, the zinc salt solution is a zinc sulfate solution, and the alkaline solution is a sodium hydroxide solution.
[0017] Preferably, the preparation method of the backwater all-purpose adhesive comprises:
[0018] The silicate, calcium hydroxide, cement, carboxymethyl cellulose, calcium stearate, waterproofing agent, crosslinking agent, silicon dioxide, silica fume and nano zinc oxide are uniformly mixed according to weight ratio to obtain a dry powder mixture;
[0019] Water is added to the dry powder mixture, and then stirred to obtain a slurry of water-retaining multipurpose adhesive;
[0020] After the slurry is left to stand and mature, the backwater all-purpose adhesive can be obtained.
[0021] Preferably, water is added to the dry powder mixture by spraying water.
[0022] Preferably, water is added to the dry powder mixture, the stirring speed is 300-500 rpm, and the stirring time is 5-10 minutes.
[0023] Preferably, the temperature of the static aging is 20-30° C., and the aging time is at least 24 hours.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The back-water multipurpose adhesive disclosed in the present invention has excellent waterproof performance through a combination of specific formulas, especially using ethoxysilane as a waterproof agent. This enables the back-water multipurpose adhesive to maintain good bonding performance in a humid or underwater environment, greatly improving its application range and durability.
[0026] The formula of the back-water universal adhesive disclosed in the present invention includes a variety of inorganic materials such as silicate, calcium hydroxide, cement, etc. These materials give the back-water universal adhesive higher strength and durability. This material combination enables the back-water universal adhesive to maintain stable performance when subjected to heavy pressure or long-term stress, and is not prone to cracking or failure.
[0027] By adding water to the dry powder mixture by spraying and stirring at an appropriate stirring speed, the back-water multi-purpose adhesive can be easily operated and constructed during the construction process. At the same time, after the slurry is left to mature, a uniform and stable colloid can be obtained, further improving the construction efficiency and quality.
[0028] In the preparation process of the back water all-purpose adhesive of the present invention, no toxic and harmful substances are used, and the raw materials in the formula are mostly inorganic materials, which are environmentally friendly. At the same time, the preparation process is simple, the energy consumption is low, and it conforms to the production concept of green environmental protection. Since the back water all-purpose adhesive has excellent waterproof performance and high strength characteristics, it is widely used in various construction and decoration occasions. Whether indoors or outdoors, wet or dry environment, the back water all-purpose adhesive can provide reliable bonding effect and meet various use requirements.
[0029] In summary, the preparation of the water-repellent multipurpose adhesive with waterproof performance disclosed in the present invention has many beneficial effects, including excellent waterproof performance, high strength and durability, good construction performance, environmental protection and a wide range of applications. DETAILED DESCRIPTION
[0030] The exemplary embodiments of the present disclosure will be described in more detail below. Although the following content shows exemplary embodiments of the present disclosure, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present disclosure and to be able to fully convey the scope of the present disclosure to those skilled in the art. It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0031] The present invention relates to the field of building materials, in particular to a back-water all-purpose adhesive with waterproof performance. With the continuous development of modern building technology, the requirements for building materials are also increasing, especially in terms of waterproof performance. The present invention aims to provide a back-water all-purpose adhesive with superior performance and convenient use through a carefully designed formula and preparation process to meet market demand.
[0032] The back-water multipurpose adhesive of the present invention is mainly composed of the following components: silicate, calcium hydroxide, cement, carboxymethyl cellulose, calcium stearate, waterproofing agent, cross-linking agent, silicon dioxide, silica fume, nano zinc oxide and water. The selection and proportion of these components are carefully prepared to ensure that the back-water multipurpose adhesive has excellent waterproof performance and bonding strength.
[0033] Among them, silicate, calcium hydroxide and cement are used as substrates to provide the main structure of the back water universal adhesive. Carboxymethyl cellulose, as a thickener and stabilizer, can enhance the viscosity and stability of the colloid. Calcium stearate is used as a lubricant to improve the construction performance of the colloid. Waterproofing agent and crosslinking agent are key components of the present invention, which can significantly improve the waterproof performance of the back water universal adhesive and enhance the bonding force between the colloid and the substrate. Silicon dioxide, silica fume and nano zinc oxide are used as reinforcing agents to further improve the strength and durability of the back water universal adhesive.
[0034] Regarding the preferred embodiment of each component, the particle size of silicon dioxide is selected to be 60-100 mesh, which can not only ensure its uniform distribution in the colloid, but also give full play to its reinforcing effect. The waterproofing agent is selected from ethoxysilane, which has excellent waterproof performance and durability, and can effectively improve the waterproof effect of the back water multi-purpose adhesive. The cross-linking agent is selected from diisocyanate, which can react chemically with other components in the colloid to form a cross-linking structure, further improving the strength and stability of the colloid.
[0035] Regarding the preparation methods of each component, the preparation process of carboxymethyl cellulose includes the steps of dissolving wood cellulose, reacting to obtain sodium carboxymethyl cellulose, acidifying with hydrochloric acid, washing and drying. The preparation process of nano zinc oxide includes the steps of reacting a zinc salt solution with an alkaline solution to generate zinc hydroxide precipitate, pyrolyzing to obtain zinc oxide particles, and calcining to obtain nano zinc oxide. The selection of these preparation methods is based on the consideration that the process is simple, the cost is low, and it is easy to realize industrial production.
[0036] In the preparation method of the back water universal adhesive, firstly, the components are mixed uniformly according to the weight ratio to obtain a dry powder mixture, and then water is added to the dry powder mixture by spraying and stirring to obtain a slurry of the back water universal adhesive. After standing and aging, the back water universal adhesive can be obtained. Among them, the stirring speed is controlled at 300-500 rpm, and the stirring time is 5-10 minutes to ensure that the components are fully mixed. The temperature of standing and aging is controlled at 20-30°C, and the aging time is at least 24 hours to ensure that the back water universal adhesive is fully matured and achieves the best performance.
[0037] In summary, the waterproof backwater all-purpose adhesive proposed by the present invention achieves excellent waterproof performance and bonding strength through a carefully designed formula and preparation process. The backwater all-purpose adhesive is not only suitable for waterproofing projects in various humid environments, but also has the advantages of convenient construction, stable performance, good durability, etc., and has broad market application prospects. At the same time, the preparation method of the present invention is simple and easy to implement, has low cost, and is easy to realize industrial production, which is of great significance for promoting the development of the building materials industry.
[0038] The technical solution of the present invention is described below through specific embodiments.
[0039] Example 1 Preparation of water-resistant multipurpose adhesive
[0040] 1. Raw materials
[0041] 25 parts of silicate, 15 parts of calcium hydroxide, 35 parts of cement, 4 parts of carboxymethyl cellulose, 2 parts of calcium stearate, 7 parts of waterproofing agent, 3 parts of cross-linking agent, 7 parts of silicon dioxide, 8 parts of silica fume, 2 parts of nano zinc oxide and 20 parts of water.
[0042] The particle size of silicon dioxide is 60-100 meshes, the waterproofing agent is ethoxysilane, and the cross-linking agent is diisocyanate.
[0043] The preparation method of carboxymethyl cellulose comprises: dissolving wood cellulose in a mixed solution of sodium hydroxide and chloroacetic acid to react to obtain sodium carboxymethyl cellulose, and then acidifying with hydrochloric acid, washing and drying to obtain carboxymethyl cellulose.
[0044] The preparation method of nano zinc oxide includes: reacting zinc sulfate solution with sodium hydroxide solution to generate zinc hydroxide precipitate, and then pyrolyzing at 450°C to obtain zinc oxide particles; calcining the zinc oxide particles at 600°C, and cooling to obtain nano zinc oxide, wherein the particle size of the nano zinc oxide is 10-100nm.
[0045] 2. Preparation
[0046] Mixing silicate, calcium hydroxide, cement, carboxymethyl cellulose, calcium stearate, ethoxysilane, diisocyanate, silicon dioxide, silica fume and nano zinc oxide uniformly according to weight ratio to obtain a dry powder mixture;
[0047] Adding water to the dry powder mixture by spraying water, and then stirring at a stirring speed of 400 rpm for 7 minutes to obtain a slurry of water-backed all-purpose adhesive;
[0048] The slurry is allowed to stand and mature for 28 hours at 25° C. to obtain the backwater all-purpose adhesive.
[0049] Example 2 Preparation of water-resistant multipurpose adhesive
[0050] 1. Raw materials
[0051] 20 parts of silicate, 10 parts of calcium hydroxide, 30 parts of cement, 2 parts of carboxymethyl cellulose, 1 part of calcium stearate, 5 parts of waterproofing agent, 2 parts of cross-linking agent, 5 parts of silicon dioxide, 5 parts of silica fume, 1 part of nano zinc oxide and 18-24 parts of water.
[0052] The particle size of silicon dioxide is 60-100 meshes, the waterproofing agent is ethoxysilane, and the cross-linking agent is diisocyanate.
[0053] The preparation method of carboxymethyl cellulose comprises: dissolving wood cellulose in a mixed solution of sodium hydroxide and chloroacetic acid to react to obtain sodium carboxymethyl cellulose, and then acidifying with hydrochloric acid, washing and drying to obtain carboxymethyl cellulose.
[0054] The preparation method of nano zinc oxide includes: reacting zinc sulfate solution with sodium hydroxide solution to generate zinc hydroxide precipitate, and then pyrolyzing at 300°C to obtain zinc oxide particles; calcining the zinc oxide particles at 400°C, and cooling to obtain nano zinc oxide, wherein the particle size of the nano zinc oxide is 10-100nm.
[0055] 2. Preparation
[0056] Mixing silicate, calcium hydroxide, cement, carboxymethyl cellulose, calcium stearate, ethoxysilane, diisocyanate, silicon dioxide, silica fume and nano zinc oxide uniformly according to weight ratio to obtain a dry powder mixture;
[0057] Adding water to the dry powder mixture by spraying water, and then stirring at a stirring speed of 300 rpm for 5 minutes to obtain a slurry of water-backed all-purpose adhesive;
[0058] The slurry is allowed to stand and mature for 24 hours at 20° C. to obtain the backwater all-purpose adhesive.
[0059] Example 3 Preparation of water-resistant multipurpose adhesive
[0060] 1. Raw materials
[0061] 30 parts of silicate, 20 parts of calcium hydroxide, 40 parts of cement, 5 parts of carboxymethyl cellulose, 3 parts of calcium stearate, 10 parts of waterproofing agent, 5 parts of cross-linking agent, 10 parts of silicon dioxide, 10 parts of silica fume, 3 parts of nano zinc oxide and 24 parts of water.
[0062] The particle size of silicon dioxide is 60-100 meshes, the waterproofing agent is ethoxysilane, and the cross-linking agent is diisocyanate.
[0063] The preparation method of carboxymethyl cellulose comprises: dissolving wood cellulose in a mixed solution of sodium hydroxide and chloroacetic acid to react to obtain sodium carboxymethyl cellulose, and then acidifying with hydrochloric acid, washing and drying to obtain carboxymethyl cellulose.
[0064] The preparation method of nano zinc oxide includes: reacting zinc sulfate solution with sodium hydroxide solution to generate zinc hydroxide precipitate, and then pyrolyzing at 600°C to obtain zinc oxide particles; calcining the zinc oxide particles at 800°C, and obtaining nano zinc oxide after cooling, wherein the particle size of the nano zinc oxide is 10-100nm.
[0065] 2. Preparation
[0066] Mixing silicate, calcium hydroxide, cement, carboxymethyl cellulose, calcium stearate, ethoxysilane, diisocyanate, silicon dioxide, silica fume and nano zinc oxide uniformly according to weight ratio to obtain a dry powder mixture;
[0067] Adding water to the dry powder mixture by spraying water, and then stirring at a stirring speed of 500 rpm for 10 min to obtain a slurry of water-backed all-purpose adhesive;
[0068] The slurry is allowed to stand and mature for 32 hours at 30° C. to obtain the backwater all-purpose adhesive.
[0069] Example 4 Preparation of Waterproof Back Water-Proof Multipurpose Adhesive
[0070] 1. Raw materials
[0071] 20 parts of silicate, 15 parts of calcium hydroxide, 34 parts of cement, 5 parts of carboxymethyl cellulose, 1 part of calcium stearate, 5 parts of waterproofing agent, 5 parts of cross-linking agent, 8 parts of silicon dioxide, 5 parts of silica fume, 1 part of nano zinc oxide and 18 parts of water.
[0072] The particle size of silicon dioxide is 60-100 meshes, the waterproofing agent is ethoxysilane, and the cross-linking agent is diisocyanate.
[0073] The preparation method of carboxymethyl cellulose comprises: dissolving wood cellulose in a mixed solution of sodium hydroxide and chloroacetic acid to react to obtain sodium carboxymethyl cellulose, and then acidifying with hydrochloric acid, washing and drying to obtain carboxymethyl cellulose.
[0074] The preparation method of nano zinc oxide includes: reacting zinc sulfate solution with sodium hydroxide solution to generate zinc hydroxide precipitate, and then pyrolyzing at 300°C to obtain zinc oxide particles; calcining the zinc oxide particles at 800°C, and cooling to obtain nano zinc oxide, wherein the particle size of the nano zinc oxide is 10-100nm.
[0075] 2. Preparation
[0076] Mixing silicate, calcium hydroxide, cement, carboxymethyl cellulose, calcium stearate, ethoxysilane, diisocyanate, silicon dioxide, silica fume and nano zinc oxide uniformly according to weight ratio to obtain a dry powder mixture;
[0077] Adding water to the dry powder mixture by spraying water, and then stirring at a stirring speed of 300 rpm for 5 minutes to obtain a slurry of water-backed all-purpose adhesive;
[0078] The slurry is allowed to stand and mature for 24 hours at 20° C. to obtain the backwater all-purpose adhesive.
[0079] Example 5 Preparation of water-resistant back multipurpose adhesive
[0080] 1. Raw materials
[0081] 20 parts of silicate, 10 parts of calcium hydroxide, 40 parts of cement, 5 parts of carboxymethyl cellulose, 3 parts of calcium stearate, 10 parts of waterproofing agent, 2 parts of cross-linking agent, 7 parts of silicon dioxide, 7 parts of silica fume, 3 parts of nano zinc oxide and 24 parts of water.
[0082] The particle size of silicon dioxide is 60-100 meshes, the waterproofing agent is ethoxysilane, and the cross-linking agent is diisocyanate.
[0083] The preparation method of carboxymethyl cellulose comprises: dissolving wood cellulose in a mixed solution of sodium hydroxide and chloroacetic acid to react to obtain sodium carboxymethyl cellulose, and then acidifying with hydrochloric acid, washing and drying to obtain carboxymethyl cellulose.
[0084] The preparation method of nano zinc oxide includes: reacting zinc sulfate solution with sodium hydroxide solution to generate zinc hydroxide precipitate, and then pyrolyzing at 500°C to obtain zinc oxide particles; calcining the zinc oxide particles at 700°C, and obtaining nano zinc oxide after cooling, wherein the particle size of the nano zinc oxide is 10-100nm.
[0085] 2. Preparation
[0086] Mixing silicate, calcium hydroxide, cement, carboxymethyl cellulose, calcium stearate, ethoxysilane, diisocyanate, silicon dioxide, silica fume and nano zinc oxide uniformly according to weight ratio to obtain a dry powder mixture;
[0087] Adding water to the dry powder mixture by spraying water, and then stirring at a stirring speed of 450 rpm for 10 min to obtain a slurry of water-backed all-purpose adhesive;
[0088] The slurry is allowed to stand and mature for 26 hours at 25° C. to obtain the backwater all-purpose adhesive.
[0089] Example 6 Preparation of water-resistant multipurpose adhesive
[0090] 1. Raw materials
[0091] 25 parts of silicate, 10 parts of calcium hydroxide, 30 parts of cement, 5 parts of carboxymethyl cellulose, 1 part of calcium stearate, 10 parts of waterproofing agent, 5 parts of cross-linking agent, 7 parts of silicon dioxide, 10 parts of silica fume, 3 parts of nano zinc oxide and 18 parts of water.
[0092] The particle size of silicon dioxide is 60-100 meshes, the waterproofing agent is ethoxysilane, and the cross-linking agent is diisocyanate.
[0093] The preparation method of carboxymethyl cellulose comprises: dissolving wood cellulose in a mixed solution of sodium hydroxide and chloroacetic acid to react to obtain sodium carboxymethyl cellulose, and then acidifying with hydrochloric acid, washing and drying to obtain carboxymethyl cellulose.
[0094] The preparation method of nano zinc oxide includes: reacting zinc sulfate solution with sodium hydroxide solution to generate zinc hydroxide precipitate, and then pyrolyzing at 400°C to obtain zinc oxide particles; calcining the zinc oxide particles at 600°C, and obtaining nano zinc oxide after cooling, wherein the particle size of the nano zinc oxide is 10-100nm.
[0095] 2. Preparation
[0096] Mixing silicate, calcium hydroxide, cement, carboxymethyl cellulose, calcium stearate, ethoxysilane, diisocyanate, silicon dioxide, silica fume and nano zinc oxide uniformly according to weight ratio to obtain a dry powder mixture;
[0097] Adding water to the dry powder mixture by spraying water, and then stirring at a stirring speed of 500 rpm for 10 min to obtain a slurry of water-backed all-purpose adhesive;
[0098] The slurry is allowed to stand and mature for 24 hours at 28° C. to obtain the backwater all-purpose adhesive.
[0099] Test Example 1
[0100] The performance test of the waterproof all-purpose adhesive prepared in Examples 1-6 was carried out, and the performance test included:
[0101] Tensile strength test, shear strength test, water resistance test and weather resistance test. The following are the specific test methods and results:
[0102] 1. Tensile strength test:
[0103] The tensile strength test of the water-repellent adhesive prepared in Examples 1-6 was performed using a universal material testing machine. During the test, the water-repellent adhesive was applied to two standard test blocks, and the test blocks were fixed on the testing machine after drying. The test blocks were stretched at a certain speed, and the maximum tensile force of the water-repellent adhesive during the stretching process was recorded. The test results show that the tensile strength of the water-repellent adhesive prepared in Examples 1-6 exceeded the standard requirements (ASTM D638), showing good tensile properties.
[0104] 2. Shear strength test:
[0105] In order to test the shear strength of the back water universal adhesive, we applied the back water universal adhesive on the contact surface of two standard test blocks, fixed the test blocks on the shear tester after drying, and sheared them at a certain speed, and recorded the maximum shear force of the back water universal adhesive during the shearing process. The test results show that the shear strength of the back water universal adhesive prepared in Examples 1-6 meets the standard requirements (ASTM D1002), showing excellent shear performance.
[0106] 3. Water resistance test:
[0107] In order to evaluate the water resistance of the back water universal adhesive, we applied the back water universal adhesive prepared in Examples 1-6 on a standard test block, then immersed it in water to observe the changes of the back water universal adhesive. After 24 hours of immersion, we found that the back water universal adhesive did not undergo obvious softening, swelling or shedding in water, showing good water resistance.
[0108] 4. Weather resistance test:
[0109] In order to test the weather resistance of the back water all-purpose adhesive, we applied the back water all-purpose adhesive prepared in Examples 1-6 on a standard test block, and then placed it in an outdoor natural environment, subject to severe weather conditions such as wind, rain, sun and rain. After 1000 hours of testing, we found that the back water all-purpose adhesive can still maintain its original performance under severe weather conditions, without obvious aging, cracking or falling off, showing excellent weather resistance.
[0110] In summary, the present invention obtains a back-water all-purpose adhesive with excellent waterproof performance through the preparation process of Examples 1-6. This adhesive shows excellent performance in multiple key performance indicators, including tensile strength, shear strength, water resistance and weather resistance. The improvement of these properties enables the back-water all-purpose adhesive to cope with various complex and changeable environmental conditions and meet a wide range of usage needs.
[0111] First, in terms of tensile strength and shear strength, this water-backed all-purpose adhesive exhibits extremely high performance. After precise experimental testing, we found that its tensile strength far exceeds that of similar products, which means that it can maintain better stability and durability when subjected to tensile forces. At the same time, its shear strength is also very good, and it can maintain a strong bond under various shear forces, ensuring that the bonded objects are not easy to fall off or be damaged when subjected to external forces.
[0112] Secondly, in terms of water resistance, the back-water multipurpose adhesive also performs well. After a long period of water immersion test, we found that it can still maintain good bonding performance without obvious softening, swelling or falling off. This is due to our careful selection of waterproof materials and unique process processing during the preparation process, which enables the glue to maintain excellent performance in humid or underwater environments.
[0113] In addition, in terms of weather resistance, the water-repellent multipurpose adhesive also demonstrates strong adaptability. Whether in harsh environments such as high temperature, low temperature, ultraviolet radiation or humidity, it can maintain stable performance without obvious aging, cracking or failure. This allows it to be used for a long time in various outdoor environments, providing reliable protection for various application scenarios.
[0114] In summary, the waterproof backwater all-purpose adhesive obtained through the preparation process of Examples 1-6 exhibits excellent performance in many aspects. Its high tensile strength, high shear strength, excellent water resistance and excellent weather resistance enable it to cope with various complex and changeable environmental conditions and meet a wide range of usage needs. Whether in the fields of home decoration, construction engineering or industrial manufacturing, this backwater all-purpose adhesive can play an excellent role and bring convenience and benefits to people's lives and work.
[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A water-resistant all-purpose adhesive. It is characterized in that In parts by weight, it includes the following components: 20-30 parts of silicate, 10-20 parts of calcium hydroxide, 30-40 parts of cement, 2-5 parts of carboxymethyl cellulose, 1-3 parts of calcium stearate, 5-10 parts of waterproofing agent, 2-5 parts of cross-linking agent, 5-10 parts of silicon dioxide, 5-10 parts of silica fume, 1-3 parts of nano zinc oxide and 18-24 parts of water.
2. The water-resistant all-purpose adhesive according to claim 1, It is characterized in that The particle size of the silicon dioxide is 60-100 meshes.
3. The water-resistant all-purpose adhesive according to claim 1, It is characterized in that The waterproofing agent is ethoxysilane; And / or, the cross-linking agent is diisocyanate.
4. The water-resistant all-purpose adhesive according to claim 1, It is characterized in that The preparation method of the carboxymethyl cellulose comprises: The lignocellulose is dissolved in a mixed solution of sodium hydroxide and chloroacetic acid to react to obtain sodium carboxymethyl cellulose, which is then acidified with hydrochloric acid, washed and dried to obtain the carboxymethyl cellulose.
5. The water-resistant all-purpose adhesive according to claim 1, It is characterized in that The preparation method of the nano zinc oxide comprises: The zinc salt solution is reacted with an alkaline solution to generate zinc hydroxide precipitate, which is then pyrolyzed at 300-600°C to obtain zinc oxide particles; The zinc oxide particles are calcined at 400-800° C. and then cooled to obtain the nano zinc oxide.
6. The water-resistant all-purpose adhesive according to claim 5, It is characterized in that The zinc salt solution is a zinc sulfate solution, and the alkaline solution is a sodium hydroxide solution.
7. The water-resistant all-purpose adhesive according to claim 1, It is characterized in that The preparation method of the backwater all-purpose adhesive comprises: The silicate, calcium hydroxide, cement, carboxymethyl cellulose, calcium stearate, waterproofing agent, crosslinking agent, silicon dioxide, silica fume and nano zinc oxide are uniformly mixed according to weight ratio to obtain a dry powder mixture; Water is added to the dry powder mixture, and then stirred to obtain a slurry of water-retaining multipurpose adhesive; After the slurry is left to stand and mature, the backwater all-purpose adhesive can be obtained.
8. The water-resistant all-purpose adhesive according to claim 7, It is characterized in that Water is added to the dry powder mixture by spraying water.
9. The water-resistant all-purpose adhesive according to claim 7, It is characterized in that Water is added to the dry powder mixture, the stirring speed is 300-500 rpm, and the stirring time is 5-10 minutes.
10. The waterproof all-purpose adhesive according to claim 7, It is characterized in that The temperature of the static aging is 20-30° C., and the aging time is at least 24 hours.