Sulfur in-situ blocking waste tire full-component recovery method

Using sulfur in-situ blocking technology to adsorb and separate sulfur-containing substances during the pyrolysis process of waste tires solves the problems of low heat utilization and difficult pollution control, and achieves efficient recovery of valuable components and reduction of pollution.

CN118772907APending Publication Date: 2024-10-15BEIJING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410916063.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the pyrolysis process of waste tires, there are problems such as low heat utilization, difficulty in controlling sulfur pollutants, and low utilization of valuable components.

Method used

Using sulfur in-situ blocking technology, attapulgite is modified at high temperature and then immersed in DETA ethanol solution to prepare sulfur in-situ blocking agent, combined with a pyrolysis furnace to pyrolyze waste tire rubber particles under anaerobic conditions, using sulfur The in-situ blocker adsorbs sulfur-containing substances and separates the pyrolysis oil and gas phase products through the alkali spray tower. The sulfur in-situ blocker is further reused in the stripping and regeneration stage to achieve efficient directional separation.

Benefits of technology

It improves the efficient directional adsorption and recycling of sulfur-containing pollutants during the pyrolysis process of waste tires, saves energy, avoids the emission of sulfur-containing pollutants, and achieves high-value recycling and pollution reduction of valuable components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772907A_ABST
    Figure CN118772907A_ABST
Patent Text Reader

Abstract

The invention provides a sulfur in-situ blocking waste tire full-component recovery method, and relates to the technical field of waste material recycling, the method comprises the following steps: S1, preparing a sulfur in-situ blocking agent; s2, pyrolyzing the waste tire colloidal particles; s3, feeding the pyrolysis oil-gas mixture into an alkali liquor spraying tower, further feeding a gas-phase product into an oil supplementing device, and finally obtaining pyrolysis gas, pyrolysis oil and sodium sulfide; and S4, carrying out air stripping regeneration on the reacted sulfur in-situ blocking agent. According to the invention, in-situ adsorption of the pollution element sulfur in the pyrolysis process of the waste tire colloidal particles can be realized, and meanwhile, efficient directional separation of pyrolysis oil gas can be realized; and through a pyrolysis process and a sulfur blocking agent adsorption process, all-component high-value recycling and pollution monitoring of the waste tire colloidal particles are realized. The method has the advantages of being high in recycling rate, small in environmental pollution, high in separation efficiency, wide in application prospect and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste material recycling, in particular to a method for recycling all components of waste tires by sulfur in-situ blocking. Background Art

[0002] Waste tires are the fastest growing type of solid waste in urban garbage. Chinese research institutions have conducted a lot of research on the resource recycling of waste tires. The current mainstream recycling methods include mechanical recycling, chemical recycling, energy recovery and other methods. The recycling of waste tires can reduce the exploitation and consumption of natural resources and effectively reduce environmental pollution. At the same time, waste tires can be used for road construction facilities and various building materials. Mechanical recycling can be used to build road shock absorption equipment and protective walls. At present, there are still problems that need to be solved in different recycling methods for waste tires. For example, the physical recycling process is prone to produce hydrogen sulfide pollution, chemical recycling is prone to cause environmental pollution, and the solvent recycling efficiency is low. The pyrolysis method is prone to produce sulfur-containing polluted gases, the utilization rate of valuable components is low, and the tail gas treatment equipment is costly and inefficient.

[0003] The pyrolysis method for recycling waste tires has obvious advantages, and can achieve the full recycling and reuse of all valuable components in waste tires. However, the recycling of waste tires requires professional recycling and processing, and requires a professional recycling system, including collection-transportation-sorting-processing and other links. However, during the pyrolysis process, sulfur-containing pollutants are discharged into the environment, which is very easy to pollute the environment. The treatment process is complicated and the recycling is difficult. Summary of the invention

[0004] In order to solve the problems of low heat utilization rate, difficult control of sulfur-containing pollutants, and low utilization rate of valuable components in the current waste tire pyrolysis process, the present invention proposes a method for recovering all components of waste tires with in-situ sulfur blocking. The present invention can achieve in-situ adsorption of sulfur-containing pollutants in the waste tire pyrolysis process through in-situ sulfur cutting technology, and the difficulty of pollutant treatment is reduced. The pyrolysis method can achieve directional separation and recovery of organic matter in waste tires, and high-value recycling of pyrolysis oil and pyrolysis gas. The pyrolysis slag of waste tire rubber pellets is mainly carbon black, which can be used for building materials and construction facilities. The pyrolysis gas can be reused in the pyrolysis stage of waste tire rubber pellets, and the high-temperature nitrogen and a small amount of water vapor flowing out of the pyrolysis furnace in step S2 can be used in the stripping regeneration stage of the sulfur in-situ blocking agent. The high-temperature gas generated in step S2 can be used to heat the eluent (alkaline solution) to prevent the alkali solution from becoming viscous. Specifically, the technical scheme of the present invention is as follows:

[0005] A method for recycling all components of waste tires with sulfur in-situ blocking, comprising:

[0006] Step S1, preparation of sulfur in-situ blocking agent: high temperature modification of attapulgite, and then immersion of the modified attapulgite in an ethanol solution containing DETA (diethylenetriamine) to obtain the sulfur in-situ blocking agent;

[0007] Step S2, pyrolysis of waste tire rubber particles: waste tire rubber particles and sulfur in-situ blocking agents are placed in a pyrolysis furnace respectively, and the blocking agents are placed relatively downwind of the N2 flow of the waste tire rubber particles (N2 flow direction), and the ratio of waste tire rubber particles to blocking agents is 3-4:1. N2 is introduced to maintain an oxygen-free environment in the furnace and control the heating rate, and carbon black and a pyrolysis oil and gas mixture are obtained through two-stage pyrolysis; the waste tire rubber particles are converted into a mixture of carbon black and oil and gas under oxygen-free and high-temperature conditions, and the sulfur in-situ blocking agent adsorbs sulfur-containing substances in the oil and gas mixture;

[0008] Step S3, sending the pyrolysis oil-gas mixture into an alkaline liquid spray tower, adsorbing and condensing the acidic substances in the oil-gas mixture, and performing oil-gas separation (i.e., separating the pyrolysis oil and the gas phase product); the gas phase product is further sent to an oil replenisher; finally, pyrolysis gas, pyrolysis oil and sodium sulfide are obtained; obviously, due to the in-situ adsorption of the sulfur in-situ blocking agent, the amount of sodium sulfide obtained here is relatively small; in addition to the pyrolysis gas, the gas phase product also contains a part of the pyrolysis oil that has not been condensed, and the pyrolysis oil is further separated by the oil replenisher;

[0009] Step S4, the sulfur in-situ blocking agent after the reaction is blown off and regenerated, and the part with good desulfurization performance after regeneration is returned to the waste tire rubber pellet pyrolysis step, and the part with poor desulfurization performance is blown off again and regenerated.

[0010] Furthermore, in step S1, the attapulgite is modified at 300-500°C for 2-3h; when preparing the sulfur in-situ blocking agent, the amount of raw materials is: modified attapulgite: ethanol = 5-10kg: 30-60L, the mass percentage of DETA is 5-45% (DETA mass / high temperature modified attapulgite + DETA mass); the specific surface area range of the sulfur in-situ blocking agent is 0.05-20.1m 2 / g.

[0011] Furthermore, in step S2, the following two-stage pyrolysis program is adopted: the temperature of the first stage pyrolysis is 200-300°C, the pyrolysis time is 60 minutes, and the temperature of the second stage pyrolysis is 350-550°C, and the pyrolysis time is 120 minutes.

[0012] Furthermore, in step S3, the alkali solution is a 2-7wt% sodium hydroxide solution; and the acidic substance is H2S.

[0013] Furthermore, in step S3, the generated pyrolysis gas is returned to the waste tire rubber pellet pyrolysis process to provide heat.

[0014] Furthermore, in step S4, the regeneration gas in the stripping regeneration process is selected from a mixture of N2 and water vapor, wherein the flow ratio of N2 to water vapor is 100-220:60; and the stripping regeneration time is 0.5~2h.

[0015] The beneficial effects brought about by the technical solution provided by the embodiment of the present invention include at least:

[0016] Waste tire rubber particles are typical composite solid wastes. Based on the pyrolysis characteristics of its organic matter, waste tire rubber particles are pyrolyzed in a tubular pyrolysis furnace. The generated pyrolysis oil-gas mixture is further processed to obtain sodium sulfide, and the pyrolysis gas continuously supplies energy to the system. An efficient directional separation method for the preparation of sulfur in-situ blockers - regeneration - pyrolysis of waste tire rubber particles - blocker stripping regeneration - oil-gas mixture reuse is developed to achieve efficient directional recovery and utilization of valuable components in pyrolysis products. Compared with traditional processes, this method achieves efficient directional adsorption of sulfur-containing pollutants during the pyrolysis of waste tires, and the heat generated by the pyrolysis flue gas is reused in the alkali solution spraying and sulfur blocker stripping regeneration stages, saving a lot of energy and avoiding the emission of sulfur-containing pollutants into the air to pollute the environment. It not only achieves high-value recovery and utilization of valuable components in waste tire rubber particles, but also achieves pollution reduction and control. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0018] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0019] The technical solution of the present invention is described below in conjunction with the accompanying drawings.

[0020] In the embodiments of the present invention, words such as "exemplarily" and "for example" are used to indicate examples, illustrations or explanations. Any embodiment or design described as "example" in the present invention should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of the word "example" is intended to present the concept in a specific way. In addition, in the embodiments of the present invention, the meaning expressed by "and / or" can be both, or it can be either of the two.

[0021] In the embodiments of the present invention, "image" and "picture" can sometimes be used interchangeably. It should be noted that when the difference between them is not emphasized, the meanings they want to express are the same. "of", "corresponding" and "corresponding" can sometimes be used interchangeably. It should be noted that when the difference between them is not emphasized, the meanings they want to express are the same.

[0022] In the embodiments of the present invention, sometimes a subscript such as W1 may be mistakenly written as a non-subscript such as W1. When the difference is not emphasized, the meanings to be expressed are consistent.

[0023] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0024] Example 1

[0025] Step 1: The attapulgite is modified at 400°C for 2h, and then 10kg of the modified attapulgite is immersed in 50L of ethanol solution containing DETA to obtain a sulfur in-situ blocker. The mass percentage of DETA loaded is 35%, and the specific surface area of ​​the sulfur in-situ blocker is 0.2m 2 / g;

[0026] Step 2: Place waste tire rubber particles and sulfur in-situ blocking agent in a pyrolysis furnace, introduce N2 at a mass percentage of 3:1 to maintain an oxygen-free environment in the furnace and control the heating rate, and control the pyrolysis conditions: the first stage pyrolysis temperature is 300°C, the pyrolysis time is 60 minutes, the second stage pyrolysis temperature is 550°C, and the pyrolysis time is 120 minutes, to obtain a mixture of carbon black and pyrolysis oil and gas;

[0027] Step 3: The pyrolysis oil and gas mixture produced after pyrolysis is sent to an alkaline solution spray tower, and the sulfur-containing gas H2S is absorbed by a 5wt% sodium hydroxide solution to produce Na2S. The solution is evaporated by the heat of the flue gas boiler to obtain Na2S and separate the pyrolysis gas and pyrolysis oil at the same time;

[0028] Step 4: regenerate the sulfur in-situ blocking agent that adsorbs sulfur by stripping with water vapor and N2, with the rate of water vapor being 60 mL / min, the rate of N2 being 220 mL / min, and the stripping time being 2 h;

[0029] In this implementation, the removal rate of sulfur-containing pollutants was 99%, and the recycling rate of sulfur in-situ blocking agents was 98.2%.

[0030] Example 2

[0031] Step 1: The attapulgite is modified at 500°C for 2h, and then 7kg of the modified attapulgite is immersed in 60L of ethanol solution containing DETA to obtain a sulfur in-situ blocker. The mass percentage of the loaded DETA is 45%, and the specific surface area of ​​the sulfur in-situ blocker is 0.05m 2 / g;

[0032] Step 2: Place waste tire rubber particles and sulfur in-situ blocking agent in a pyrolysis furnace with a mass percentage of 4:1, introduce N2 to maintain an oxygen-free environment in the furnace and control the heating rate and pyrolysis conditions: the first stage pyrolysis temperature is 300°C and the pyrolysis time is 60 minutes, the second stage pyrolysis temperature is 450°C and the pyrolysis time is 120 minutes, and a mixture of carbon black and pyrolysis oil and gas is obtained;

[0033] Step 3: The pyrolysis oil and gas mixture produced after pyrolysis is sent to an alkaline solution spray tower, and the sulfur-containing gas H2S is absorbed by a 7wt% sodium hydroxide solution to produce Na2S. The solution is evaporated by the heat of the flue gas boiler to obtain Na2S and separate the pyrolysis gas and pyrolysis oil at the same time;

[0034] Step 4: regenerate the sulfur in-situ blocking agent that adsorbs sulfur by stripping with water vapor and N2, with the rate of water vapor being 60 mL / min, the rate of N2 being 160 mL / min, and the stripping time being 2 h;

[0035] In this implementation, the removal rate of sulfur-containing pollutants was 99.2%, and the recycling rate of sulfur in-situ blocking agents was 92.5%.

[0036] Comparative Example 1

[0037] Step 1: The attapulgite is modified at 300°C for 3h, and then 5kg of the modified attapulgite is immersed in 30L of ethanol solution containing DETA to obtain a sulfur in-situ blocker. The mass percentage of the loaded DETA is 5%, and the specific surface area of ​​the sulfur in-situ blocker is 20.1m 2 / g;

[0038] Step 2: Place waste tire rubber particles and sulfur in-situ blocking agent in a pyrolysis furnace with a mass percentage of 4:1, introduce N2 to maintain an oxygen-free environment in the furnace and control the heating rate, and control the pyrolysis conditions: the first stage pyrolysis temperature is 200°C, the pyrolysis time is 60 minutes, the second stage pyrolysis temperature is 350°C, and the pyrolysis time is 120 minutes, to obtain a mixture of carbon black and pyrolysis oil and gas;

[0039] Step 3: The pyrolysis oil and gas mixture produced after pyrolysis is sent to an alkaline solution spray tower, and the sulfur-containing gas H2S is absorbed by a 5wt% sodium hydroxide solution to produce Na2S. The solution is evaporated by the heat of the flue gas boiler to obtain Na2S and separate the pyrolysis gas and pyrolysis oil at the same time;

[0040] Step 4: regenerate the sulfur in-situ blocking agent that adsorbs sulfur by stripping with water vapor and N2, the rate of water vapor is 60 mL / min, the rate of N2 is 100 mL / min, and the stripping time is 0.5 h;

[0041] In this implementation, the removal rate of sulfur-containing pollutants was 60.4%, and the recycling rate of sulfur in-situ blocking agents was 70.2%.

[0042] Comparative Example 2

[0043] Step 1: The attapulgite is modified at 300°C for 3h, and then 5kg of the modified attapulgite is immersed in 30L of ethanol solution containing DETA to obtain a sulfur in-situ blocker. The mass percentage of the loaded DETA is 10%, and the specific surface area of ​​the sulfur in-situ blocker is 10.2m 2 / g;

[0044] Step 2: Place waste tire rubber particles and sulfur in-situ blocking agent in a pyrolysis furnace with a mass percentage of 4:1, introduce N2 to maintain an oxygen-free environment in the furnace and control the heating rate and pyrolysis conditions: the first stage pyrolysis temperature is 200°C and the pyrolysis time is 60 minutes, the second stage pyrolysis temperature is 500°C and the pyrolysis time is 120 minutes, and a mixture of carbon black and pyrolysis oil and gas is obtained;

[0045] Step 3: The pyrolysis oil and gas mixture produced after pyrolysis is sent to an alkaline solution spray tower, and the sulfur-containing gas H2S is absorbed by a 2wt% sodium hydroxide solution to produce Na2S. The solution is evaporated by the heat of the flue gas boiler to obtain Na2S and separate the pyrolysis gas and pyrolysis oil at the same time;

[0046] Step 4: regenerate the sulfur in-situ blocking agent that adsorbs sulfur by stripping with water vapor and N2, with the rate of water vapor being 60 mL / min, the rate of N2 being 100 mL / min, and the stripping time being 1 h;

[0047] In this implementation, the removal rate of sulfur-containing pollutants was 76.5%, and the recycling rate of sulfur in-situ blocking agents was 75.1%.

[0048] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for recovering all components of waste tires with sulfur in-situ blocking, characterized in that: include: Step S1, preparation of sulfur in-situ blocking agent: high temperature modification of attapulgite, and then immersion of the modified attapulgite in an ethanol solution containing DETA to obtain a sulfur in-situ blocking agent; Step S2, pyrolysis of waste tire rubber particles: placing waste tire rubber particles and sulfur in-situ blocking agents in a pyrolysis furnace respectively, with the blocking agents relatively placed downwind of the N2 flow of the waste tire rubber particles, and the mass ratio of waste tire rubber particles to blocking agents is in the range of 3-4:1; introducing N2 to maintain an oxygen-free environment in the furnace and controlling the heating rate, and obtaining a mixture of carbon black and pyrolysis oil and gas through two-stage pyrolysis; Step S3, sending the pyrolysis oil-gas mixture into an alkaline solution spray tower, adsorbing and condensing the acidic substances in the oil-gas mixture, and separating the oil and gas at the same time; the gas phase product is further sent to an oil replenisher; and finally pyrolysis gas, pyrolysis oil and sodium sulfide are obtained; Step S4, the sulfur in-situ blocking agent after the reaction is blown off and regenerated, and the part with good desulfurization performance after regeneration is returned to the waste tire rubber pellet pyrolysis step, and the part with poor desulfurization performance is blown off again and regenerated.

2. The method according to claim 1, characterized in that In step S1, the attapulgite is modified at 300-500°C for 2-3 h; when preparing the sulfur in-situ blocking agent, the amount of raw materials is: modified attapulgite: ethanol = 5-10kg: 30-60L, the mass fraction of DETA is 5-45%; the specific surface area range of the sulfur in-situ blocking agent is 0.05-20.1m 2 / g.

3. The method according to claim 1, characterized in that: In step S2, the following two-stage pyrolysis program is adopted: the temperature of the first stage of pyrolysis is 200-300°C, the pyrolysis time is 60 minutes, and the temperature of the second stage of pyrolysis is 350-550°C, and the pyrolysis time is 120 minutes.

4. The method according to claim 1, characterized in that: In step S3, the alkali solution is a 2-7wt% sodium hydroxide solution; and the acidic substance is H2S.

5. The method according to claim 1, characterized in that In step S3, the generated pyrolysis gas is returned to the waste tire rubber pellet pyrolysis process to provide heat.

6. The method according to claim 1, characterized in that In step S4, the regeneration gas in the stripping regeneration process is selected from a mixture of N2 and water vapor, wherein the flow ratio of N2 to water vapor is 100-220:60; and the stripping regeneration time ranges from 0.5 to 2 hours.

7. The method according to claim 1, characterized in that The pyrolysis gas is recycled to the waste tire rubber pellet pyrolysis stage; the high-temperature nitrogen flowing out of the pyrolysis furnace in step S2 is used in the stripping regeneration stage of the sulfur in-situ blocking agent; the high-temperature gas generated in step S2 is used to heat the eluent.