Process for producing high-quality needle coke through co-carbonization of needle coke micro powder and refined pitch
By mixing refined asphalt and needle coke powder and optimizing the coking process, the problem of inconsistent coke production rates caused by different components of high-temperature coal tar is solved, the quality and utilization value of needle coke are improved, and efficient production in line with industry standards is achieved. Ultra-high power graphite electrode raw material.
Patent Information
- Application Number
- CN202410917185.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When producing needle coke in the existing technology, different compositions of high-temperature coal tar lead to inconsistent coking rates, which affects the quality of needle coke. Moreover, the particle size of needle coke powder is small, the utilization value is low, and it is difficult to effectively utilize it.
Refined asphalt obtained by pretreatment of high-temperature coal tar is mixed with needle coke powder in proportion, and needle coke is produced through an optimized coking process, including a multi-stage temperature and pressure-controlled temperature change operation in a heating furnace to form a uniform Mix the ingredients to speed up the reaction.
It improves the reaction rate of refined asphalt coke, improves the quality of needle coke products, and effectively utilizes needle coke powder to increase its added value. The needle coke produced has high flexural strength and meets industry standards.
Smart Images

Figure CN118772908A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of coal chemical technology, and in particular to a process for producing high-quality needle coke by co-carbonizing needle coke micropowder and refined asphalt. Background Art
[0002] Needle coke is a high-quality carbon material, named for its slender needle-like structure after crushing. It has good orientation, strong electrical and thermal conductivity, and is the main raw material for manufacturing ultra-high power graphite electrodes. The unique excellent performance of needle coke mainly comes from the special microscopic structure of the intermediate phase. Its fibrous directional anisotropic structure gives it a high degree of graphitization performance. Ultra-high power graphite electrodes produced with needle coke have the advantages of low resistivity, high volume density, high mechanical strength, small thermal expansion coefficient, and good thermal shock resistance.
[0003] Needle coke is the main raw material for producing ultra-high power graphite electrodes, and its quality directly affects the service life of the electrode rod. Needle coke production is a complex physical and chemical process. During the carbonization process of liquid carbon-containing compounds, the polycyclic aromatic hydrocarbons gradually pyrolyze and condense into small intermediate phase spheres that are insoluble in the mother liquor, which we call crystal nuclei. As the carbonization reaction continues, the small intermediate phase spheres continue to grow, merge, and orient, and finally solidify into a coke product with an oriented fibrous structure, namely needle coke. During the coking process, solvation reactions such as hydrogen transfer, alkylation transfer, and continuous intermolecular reactions occur between component molecules. Needle coke powder (less than 2μm) is added to refined asphalt as the original crystal nucleus of needle coke. Since the powder itself is needle coke, the process of gradual pyrolysis and condensation of polycyclic aromatic hydrocarbons into small intermediate phase spheres that are insoluble in the mother liquor can be omitted, which accelerates the reaction, reduces the reaction time of coke production, and reduces production energy consumption. The small spheres of the intermediate phase grow and fuse, and under the drive of the escaping gas and the action of shear stress, a wide-area streamlined intermediate phase is produced, and finally high-quality needle coke is obtained.
[0004] The main raw material for producing coal-based needle coke at home and abroad is high-temperature coal tar produced by coking. Then, after deep processing of high-temperature coal tar, light components are removed, and the remaining soft asphalt is used as raw material. Due to different sources of coal, the composition of high-temperature coal tar as waste is also greatly different, which directly affects the quality of needle coke when producing needle coke. The coking rate of soft asphalt produced by different high-temperature coal tars is also different during coking, which brings great difficulties to production operations and affects the quality of needle coke. Needle coke powder is the waste material produced in the process of grinding negative electrode. Because the particle size is too small, it cannot be used as negative electrode material. The utilization value is extremely low and it is generally treated as waste. Summary of the invention
[0005] The purpose of the present invention is to overcome the above shortcomings and provide a process for producing needle coke by co-carbonizing needle coke powder and refined asphalt, wherein refined asphalt obtained by pretreatment of high-temperature coal tar and needle coke powder are mixed in proportion, and the coking process is optimized to produce needle coke pre-calcined coke.
[0006] The technical solution adopted by the embodiment of the present application to solve the technical problem is:
[0007] A process for producing high-quality needle coke by co-carbonization of needle coke micropowder and refined asphalt, comprising the following process steps:
[0008] S1. Pre-treating high-temperature coal tar to obtain refined asphalt and needle coke powder, and mixing them to prepare a mixed raw material;
[0009] S2. The mixed raw materials are heated in a heating furnace, and the outlet of the heating furnace is kept at a variable temperature.
[0010] According to some embodiments of the present application, in step S1, the particle size of the needle coke powder is less than 2 μm.
[0011] According to some embodiments of the present application, in the step S1, refined asphalt and needle coke powder are mixed in two ways in a mixer at a mass ratio of 10:0 to 6:4, and a uniform mixed raw material is formed with the assistance of an agitator, and the stirring rate of the agitator is between 1000-5000 rpm.
[0012] According to some embodiments of the present application, in step S2, the outlet of the heating furnace is maintained at a variable temperature of 450-520°C.
[0013] According to some embodiments of the present application, in step S2, the temperature at the outlet of the heating furnace changes in five stages, as follows:
[0014] (1) In stage 1, the outlet temperature of the heating furnace is 495-520°C and the duration is 2.0h;
[0015] (2) In stage 2, the temperature of the material at the outlet of the heating furnace starts to drop from 495-520°C to 450-460°C, and the time is 2h;
[0016] (3) In stage 3, the temperature of the material at the outlet of the heating furnace is increased from 450-460°C to 500-520°C, and the duration is 12 hours;
[0017] (4) In stage 4, the material temperature at the outlet of the heating furnace is 500-520°C and the heating time is 12 hours;
[0018] (5) In stage 5, the material temperature at the outlet of the heating furnace is 500-520°C and the duration is 6 hours.
[0019] According to some embodiments of the present application, in sub-step (1) in step S2, the coking tower pressure in stage 1 is 0.2 MPa.
[0020] According to some embodiments of the present application, in sub-step (2) in step S2, the coking tower pressure in stage 2 is 0.4 MPa.
[0021] According to some embodiments of the present application, in sub-step (3) in step S2, the coking tower pressure in stage 3 is 0.8 MPa, and the circulation ratio is 1 to 1.1.
[0022] According to some embodiments of the present application, in sub-step (4) in step S2, the coking tower pressure in stage 4 is 0.7 MPa, and the circulation ratio is 1.1 to 1.2.
[0023] According to some embodiments of the present application, in sub-step (5) in step S2, the coking tower pressure in stage 5 is 0.05 MPa / h, and the circulation ratio is 1.2 to 1.5.
[0024] The advantages of the embodiments of the present application are:
[0025] 1. Using a mixture of refined asphalt and needle coke powder as raw materials increases the reaction rate of refined asphalt coking and improves the quality of needle coke products;
[0026] 2. The needle coke powder is effectively utilized, turning waste into treasure and increasing the added value of the needle coke powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 A process flow chart for producing high-quality needle coke by co-carbonization of needle coke powder and refined asphalt provided in an embodiment of the present application. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application.
[0030] In order to make the purpose, technical solutions and advantages of the implementation methods of this application clearer, the technical solutions in the implementation methods of this application will be clearly and completely described below in conjunction with the drawings in the implementation methods of this application. Obviously, the described implementation methods are part of the implementation methods of this application, not all of the implementation methods. Based on the implementation methods in this application, all other implementation methods obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0031] Embodiment 1:
[0032] like Figure 1 As shown, a process for producing high-quality needle coke by co-carbonizing needle coke powder and refined asphalt comprises the following steps:
[0033] S1. Pre-treating high-temperature coal tar to obtain refined asphalt and needle coke powder (1 μm) are mixed in a mixer in two ways at a mass ratio of 7:3, and with the assistance of a stirrer, a uniform mixed raw material is formed;
[0034] S2, the mixed raw materials are heated in a heating furnace, and the outlet of the heating furnace is kept at a variable temperature of 455-520°C;
[0035] S3. The temperature at the outlet of the heating furnace changes in three stages, as follows:
[0036] (1) In stage 1, the outlet material temperature of the heating furnace is 505°C, the duration is 2.0h, and the coking tower pressure is 0.2MPa;
[0037] (2) In stage 2, the temperature of the material at the outlet of the heating furnace is cooled from 505°C to 455°C, the cooling rate is 25°C / h, the time is 2h, and the coking tower pressure is 0.4MPa;
[0038] (3) In stage 3, the outlet temperature of the heating furnace is increased from 455°C to 515°C, the heating rate is 5°C / h, the duration is 12h, the coking tower pressure is 0.8MPa, and the circulation ratio is 1.1; the coking circulation ratio is the ratio of the circulating oil volume to the fresh raw oil volume. It is an important operating parameter that affects the processing capacity, product properties and distribution of the delayed coking unit.
[0039] (4) In stage 4, the outlet material temperature of the heating furnace is 515°C, the pressure of the coking tower is 0.7MPa, the circulation ratio is 1.2, and the time is 12h;
[0040] (5) In stage 5, the outlet material temperature of the heating furnace is 515°C, the duration is 6 hours, the pressure reduction rate of the coking tower is 0.05 MPa / h, and the circulation ratio is 1.5.
[0041] After calcining and graphitizing the green needle coke obtained in Example 1, a large-scale ultra-high power graphite electrode of Φ550 was produced. The flexural strength of the electrode was tested, and the flexural strength reached 19 MPa, meeting the requirement of Φ550 electrode flexural strength ≥ 10 MPa in the industry standard YB / T 4090-2015.
[0042] Embodiment 2:
[0043] like Figure 1 As shown, a process for producing high-quality needle coke by co-carbonizing needle coke powder and refined asphalt comprises the following steps:
[0044] S1. Refined asphalt and needle coke powder (1.2 μm) obtained by pretreatment of high-temperature coal tar are mixed in a mixer in two ways at a mass ratio of 8:2, and a uniform mixed raw material is formed with the aid of a stirrer;
[0045] S2, the mixed raw materials are heated in a heating furnace, and the outlet of the heating furnace is kept at a variable temperature of 465-510;
[0046] S3. The temperature at the outlet of the heating furnace changes in three stages, as follows:
[0047] (1) In stage 1, the outlet material temperature of the heating furnace is 510°C, the duration is 2.0h, and the coking tower pressure is 0.2MPa;
[0048] (2) In stage 2, the temperature of the material at the outlet of the heating furnace is cooled from 510°C to 465°C, the cooling rate is 22.5°C / h, the time is 2h, and the coking tower pressure is 0.4MPa;
[0049] (3) In stage 3, the temperature of the material at the outlet of the heating furnace is increased from 465°C to 510°C, the heating rate is 3.75°C / h, the duration is 12h, the coking tower pressure is 0.8MPa, and the circulation ratio is 1.1;
[0050] (4) In stage 4, the outlet material temperature of the heating furnace is 510°C, the pressure of the coking tower is 0.7MPa, the circulation ratio is 1.2, and the time is 12h;
[0051] (5) In stage 5, the outlet material temperature of the heating furnace is 510°C, the duration is 6 hours, the pressure reduction rate of the coking tower is 0.05 MPa / h, and the circulation ratio is 1.5.
[0052] After calcining and graphitizing the green needle coke obtained in Example 2, a large-scale ultra-high power graphite electrode of Φ550 was produced. The flexural strength of the electrode was tested, and the flexural strength reached 16MPa, meeting the requirement of Φ550 electrode flexural strength ≥10MPa in the industry standard YB / T 4090-2015.
[0053] Embodiment 3:
[0054] like Figure 1 As shown, a process for producing high-quality needle coke by co-carbonizing needle coke powder and refined asphalt comprises the following steps:
[0055] S1. Refined asphalt and needle coke powder (1.2 μm) obtained by pretreatment of high-temperature coal tar are mixed in a mixer in two ways at a mass ratio of 9:1, and with the assistance of a stirrer, a uniform mixed raw material is formed;
[0056] S2, the mixed raw materials are heated in a heating furnace, and the outlet of the heating furnace is kept at a variable temperature of 450-520°C;
[0057] S3. The temperature at the outlet of the heating furnace changes in three stages, as follows:
[0058] (1) In stage 1, the outlet material temperature of the heating furnace is 515°C, the duration is 2.0h, and the coking tower pressure is 0.2MPa;
[0059] (2) In stage 2, the outlet temperature of the heating furnace is cooled from 515°C to 450°C, the cooling rate is 32.5°C / h, the time is 2h, and the coking tower pressure is 0.4MPa;
[0060] (3) In stage 3, the outlet temperature of the heating furnace is increased from 450°C to 520°C, the heating rate is 5.83°C / h, the duration is 12h, the coking tower pressure is 0.8MPa, and the circulation ratio is 1.1;
[0061] (4) In stage 4, the outlet material temperature of the heating furnace is 520°C, the pressure of the coking tower is 0.7MPa, the circulation ratio is 1.2, and the time is 12h;
[0062] (5) In stage 5, the outlet material temperature of the heating furnace is 520°C, the duration is 6 hours, the pressure reduction rate of the coking tower is 0.05 MPa / h, and the circulation ratio is 1.5.
[0063] After calcining and graphitizing the green needle coke obtained in Example 3, a large-scale ultra-high power graphite electrode of Φ550 was produced. The flexural strength of the electrode was tested, and the flexural strength reached 21 MPa, meeting the requirement of Φ550 electrode flexural strength ≥ 10 MPa in the industry standard YB / T 4090-2015.
[0064] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.
Claims
1. A process for producing high-quality needle coke by co-carbonization of needle coke powder and refined pitch, characterized in that: The process steps include: S1. Pre-treating high-temperature coal tar to obtain refined asphalt and needle coke powder, and mixing them to prepare a mixed raw material; S2. The mixed raw materials are heated in a heating furnace, and the outlet of the heating furnace is kept at a variable temperature.
2. The process for producing high-quality needle coke by co-carbonization of needle coke powder and refined asphalt as claimed in claim 1, characterized in that: In the step S1, the particle size of the needle coke powder is less than 2 μm.
3. The process for producing high-quality needle coke by co-carbonization of needle coke micropowder and refined asphalt as claimed in claim 1, characterized in that: In the step S1, the refined asphalt and the needle coke powder are mixed in two ways in a mixer at a mass ratio of 10:0 to 6:4, and a uniform mixed raw material is formed with the assistance of a stirrer, and the stirring rate of the stirrer is between 1000 and 5000 rpm.
4. The process for producing high-quality needle coke by co-carbonization of needle coke powder and refined asphalt as claimed in claim 1, characterized in that: In step S2, the outlet of the heating furnace is kept at a variable temperature of 450-520°C.
5. The process for producing high-quality needle coke by co-carbonization of needle coke powder and refined pitch as claimed in claim 1, characterized in that: In step S2, the temperature at the outlet of the heating furnace changes in five stages, as follows: (1) In stage 1, the outlet temperature of the heating furnace is 495-520°C and the duration is 2.0h; (2) In stage 2, the temperature of the material at the outlet of the heating furnace starts to drop from 495-520°C to 450-460°C, and the time is 2h; (3) In stage 3, the temperature of the material at the outlet of the heating furnace is increased from 450-460°C to 500-520°C, and the duration is 12 hours; (4) In stage 4, the material temperature at the outlet of the heating furnace is 500-520°C and the heating time is 12 hours; (5) In stage 5, the material temperature at the outlet of the heating furnace is 500-520°C and the duration is 6 hours.
6. The process for producing high-quality needle coke by co-carbonization of needle coke powder and refined asphalt as claimed in claim 5, characterized in that: In sub-step (1) of step S2, the coking drum pressure in stage 1 is 0.2 MPa.
7. The process for producing high-quality needle coke by co-carbonization of needle coke powder and refined pitch as claimed in claim 5, characterized in that: In sub-step (2) of step S2, the coking drum pressure in stage 2 is 0.4 MPa.
8. The process for producing high-quality needle coke by co-carbonization of needle coke powder and refined pitch as claimed in claim 5, characterized in that: In sub-step (3) of step S2, the coking tower pressure in stage 3 is 0.8 MPa and the circulation ratio is 1 to 1.
1.
9. The process for producing high-quality needle coke by co-carbonization of needle coke powder and refined pitch as claimed in claim 5, characterized in that: In sub-step (4) of step S2, the coking tower pressure in stage 4 is 0.7 MPa and the circulation ratio is 1.1 to 1.
2.
10. The process for producing high-quality needle coke by co-carbonization of needle coke powder and refined pitch as claimed in claim 5, characterized in that: In sub-step (5) of step S2, the coking tower pressure in stage 5 is 0.05 MPa / h, and the circulation ratio is 1.2 to 1.5.