High-thermal-conductivity die-casting high-temperature brazing aluminum alloy and preparation method thereof

By adjusting the proportions of Si, Fe, Ce, Mg, Sr and other elements in aluminum alloys, combined with die casting and aging treatment, the problems of large material loss, high cost and low thermal conductivity of traditional aluminum alloys during high-temperature brazing are solved. Aluminum alloy material that achieves high thermal conductivity, high-quality welding and good heat dissipation.

CN118773486APending Publication Date: 2024-10-15CHONGQING HUIDING HUACHUANG INFORMATION TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410809871.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

During the high-temperature brazing process, traditional aluminum alloy materials have large material losses, long production cycles, high costs, and low thermal conductivity, which cannot meet the temperature requirements of high-temperature brazing and affect the heat dissipation effect of parts.

Method used

A high thermal conductivity die-cast high-temperature brazing aluminum alloy is used, containing Si, Fe, Ce, Mg, Sr and other elements. The component ratio is adjusted to increase the thermal conductivity and melting point. Combined with die-casting and aging treatment processes, a thermal conductivity of 180~ 215W/m.K aluminum alloy meets the temperature requirements for high-temperature brazing.

Benefits of technology

It achieves high-quality welding of aluminum alloy parts during high-temperature brazing, ensures the brazing quality and heat dissipation effect, reduces production costs, and meets the thermal conductivity requirements of the heat dissipation and temperature control module for aluminum alloy materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004905862980000071
    Figure BDA0004905862980000071
Patent Text Reader

Abstract

The invention discloses a high-thermal-conductivity die-casting high-temperature brazing aluminum alloy and a preparation method thereof.The aluminum alloy comprises, by mass, 0.2%-0.6% of Si, 0.8%-1.5% of Fe, 0.3%-1.0% of Ce, 0.1%-0.3% of Mg, 0.006%-0.02% of Sr, the balance Al and inevitable impurities. The rest elements are all impurity elements, the content of a single impurity element is less than 0.05%, the total amount of the impurity elements is less than 0.15%, and the balance is aluminum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloys, and in particular to a high thermal conductivity die-casting and high temperature brazing aluminum alloy and a preparation method thereof. Background Art

[0002] In recent years, industrial technology has developed rapidly. In many fields such as the power industry, aerospace, military, mining, and electronic products, higher computing speeds, higher operating speeds, and higher energy transfer conversions are reflected. Equipment and components generate more heat, and temperature control of equipment and components is required to reduce the temperature of the equipment and ensure smooth operation and reliability.

[0003] The heat dissipation and temperature control module is usually made of aluminum alloy 6063 (T5: thermal conductivity is 209W / mK) or 6061 (thermal conductivity is 167W / mK at T6). It is processed into parts by extruding plates or forgings, then mechanically removing materials, and then welding them through high-temperature brazing. This processing method results in large loss of raw materials, large investment in processing equipment, long processing cycle, and excessively high overall part production costs.

[0004] Traditional die-cast aluminum alloy materials ADC12 and A380 are used for die-casting rapid prototyping of parts. The melting point of this type of general conventional die-cast aluminum alloy is generally lower than 570°C. When die-casting traditional aluminum alloy materials are used to prepare aluminum alloy parts through high-temperature brazing, a large area of ​​the part body will melt, resulting in poor brazing quality. This is because traditional die-casting materials do not meet the temperature requirements of high-temperature brazing, and the brazing temperature range of high-temperature brazing is 580-610°C; at the same time, the thermal conductivity of traditional die-cast aluminum alloy ADC12 and A380 materials is lower than 100W / mK, and the thermal conductivity of the parts prepared from the corresponding aluminum alloy is not good, which affects the heat dissipation effect of the parts. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a high thermal conductivity die-cast high-temperature brazing aluminum alloy and a preparation method thereof, so as to solve the problems of large material loss, long production cycle, high production cost, and traditional die-casting materials not meeting the temperature requirements of high-temperature brazing and poor thermal conductivity in the production process of aluminum components in the prior art.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A high thermal conductivity die-casting high temperature brazing aluminum alloy, calculated by mass percentage, the aluminum alloy comprises the following components:

[0008] Si is 0.2-0.6%, Fe is 0.8-1.5%, Ce is 0.3-1.0%, Mg is 0.1-0.3%, Sr is 0.006-0.02%;

[0009] All elements other than the above elements are impurity elements, and the content of a single impurity element is less than 0.05%, the total amount of the impurity elements is less than 0.15%, and the balance is aluminum.

[0010] Preferably, in the aluminum alloy, the mass ratio of Si to Mg is (2-18):3.

[0011] Preferably, the melting point of the aluminum alloy is 640-655°C.

[0012] Preferably, the thermal conductivity of the aluminum alloy is 180-215 W / mK.

[0013] Preferably, the aluminum alloy has a tensile strength greater than 120 MPa, a yield strength greater than 60 MPa, and an elongation greater than 8%.

[0014] The present invention provides a method for preparing a high thermal conductivity die-casting high temperature brazing aluminum alloy. The specific steps for preparing the above aluminum alloy are as follows:

[0015] Step 1: preparing materials so that the proportion of each component satisfies the above-mentioned aluminum alloy; wherein the raw materials include aluminum ingots, magnesium ingots, iron additives, industrial silicon, aluminum strontium alloy, and aluminum cerium alloy;

[0016] Step 2: Place the aluminum ingot in a melting furnace and heat it to melt to obtain aluminum liquid. The temperature of the aluminum liquid is controlled at 730-780°C. Then, industrial silicon and iron additives are added. After all are melted, the temperature is lowered to 700-730°C, and a refining agent is added to refine the aluminum liquid.

[0017] Step 3: Add magnesium ingot and aluminum-cerium alloy to the aluminum liquid obtained in step 2, control the temperature at 680-700°C after all are melted, add aluminum-strontium alloy, detect its components after all are melted, perform degassing after qualified, and maintain the aluminum liquid temperature at 680-700°C;

[0018] Step 4: The aluminum obtained in step 3 is hydraulically pressed into a mold for die casting, and the obtained casting is subjected to aging treatment to obtain the high thermal conductivity die-cast high temperature brazing aluminum alloy.

[0019] Preferably, in step 4, before die-casting, the die-casting mold is kept at a temperature of 260-300° C. in advance; during die-casting, the aluminum liquid is cast in a barrel at 280-350° C. and a pressure of 65-75 MPa.

[0020] Preferably, in step 4, the aging treatment process is: aging temperature: 250-350° C.; aging insulation time: 3-4 hours.

[0021] The present invention provides an application of a high thermal conductivity die-cast high temperature brazing aluminum alloy, wherein the aluminum alloy or the aluminum alloy prepared by the preparation method is used to prepare a heat dissipation temperature control liquid cooling module assembly through brazing. The specific steps are as follows:

[0022] Step ①: using the high thermal conductivity die-casting high temperature brazing aluminum alloy of the present invention as a raw material, and die-casting aluminum alloy parts using the above steps and methods;

[0023] Step ②: Remove the riser of the die-cast aluminum alloy parts; remove burrs; perform aging heat treatment; and machine the parts;

[0024] Step 3: Degrease the brazed parts; spray fiber; dry; assemble and fix;

[0025] Step ④: In a high-purity nitrogen atmosphere; perform continuous tunnel furnace brazing; the high-temperature brazing temperature range is 590-610℃;

[0026] Step ⑤: Laser marking;

[0027] Step ⑥: Helium air tightness check;

[0028] Step 7: Component size inspection;

[0029] Step ⑧: Finished product packaging; obtaining a high thermal conductivity die-cast high temperature brazing aluminum alloy heat dissipation temperature control liquid cooling module assembly.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The present invention adjusts the raw material components of the aluminum alloy so that the prepared aluminum alloy has a high thermal conductivity and melting point on the premise that its mechanical properties meet the requirements, can meet the temperature requirements during high-temperature brazing, and the aluminum alloy component body will not melt on a large scale during high-temperature brazing, ensuring excellent quality after brazing; at the same time, it also has a high thermal conductivity, and the heat dissipation component prepared by using the aluminum alloy has a good heat dissipation effect, which can fully meet the heat dissipation requirements of the heat dissipation temperature control module for the aluminum alloy material. DETAILED DESCRIPTION

[0032] The present invention will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. All other embodiments obtained by ordinary technicians in this field based on the present invention belong to the scope of protection of the present invention.

[0033] Unless otherwise indicated in specific cases in the present invention, the numerical ranges listed herein include the upper and lower limits, and all integers and fractions within the range, and are not limited to the specific values ​​listed when defining the range.

[0034] 1. A high thermal conductivity die-casting high temperature brazing aluminum alloy

[0035] Calculated by mass percentage, the aluminum alloy includes the following components:

[0036] Si is 0.2-0.6%, Fe is 0.8-1.5%, Ce is 0.3-1.0%, Mg is 0.1-0.3%, Sr is 0.006-0.02%;

[0037] The remaining elements are all impurity elements, and the content of a single impurity element is less than 0.05%, the total amount of the impurity elements is less than 0.15%, and the balance is aluminum.

[0038] In some embodiments, Fe is the main additive element, and its dosage is controlled between 0.8% and 1.5%. In order to ensure that a certain amount of Al 3 Fe alloy phase structure, this alloy phase structure can reduce the formation of Al-Fe-Si intermediate phase, which will cause the aluminum liquid to adhere to the mold, resulting in sticking mold phenomenon during the die casting process, which is not conducive to the molding of die castings. However, too high or too little Fe element will affect Al 3 The amount of Fe alloy phase structure formed, thereby affecting the beneficial effect of this alloy phase structure. Therefore, the amount of Fe element can be 0.8%, 0.81%, 0.85%, 0.9%, 0.95%, 1.0%, 1.1%, 1.2%, 1.41%, 1.5%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0039] In some embodiments, the present invention controls the amount of Si element to be between 0.2% and 0.6%. Although Si can improve the fluidity of the die-cast aluminum alloy, too high a Si content can easily reduce the melting point of the aluminum alloy material, resulting in the aluminum alloy being difficult to meet the temperature requirements of high-temperature brazing, and thus making the aluminum alloy easy to melt during high-temperature brazing, which ultimately affects the brazing quality; however, too low a Si content is not conducive to the formation of strengthening alloy phases, especially β-AlFeSi phase and Mg 2 The formation of Si phase, β-AlFeSi phase can reduce the material structure to form long needle-shaped aluminum iron structure, reducing the deformation of metal material structure. A sufficient amount of β-AlFeSi phase in the alloy material can enhance the thermal conductivity and elongation of the material. 2 Si phase can enhance the mechanical properties of the matrix material, but Mg 2 Too much Si phase will reduce the elongation of the material, Mg 2Too little Si phase will reduce the tensile strength and yield strength of the material. At the same time, too low Si content will cause the trace Sr element to be unable to play its beneficial role, weaken the inhibition of Sr element on the hydrogen absorption of aluminum alloy, make the hydrogen absorption of aluminum alloy material serious, and then cause the aluminum alloy to easily form pores and pinholes during die casting, ultimately reducing the mechanical properties and brazing quality of the material, and also making the adverse effects of Si be amplified. Therefore, the amount of Si element can be 0.2%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.4%, 0.55%, 0.60%, etc., as well as all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0040] In some embodiments, the amount of Mg element is controlled between 0.1% and 0.3%. Mg can improve the corrosion resistance of aluminum alloy materials and improve the mechanical properties of materials. At the same time, Mg element can form a certain amount of Mg with Si. 2 Based on this, the present invention adjusts the amount of Mg element. Too high Mg content will lead to the formation of Mg 2 Too much Si phase will reduce the welding quality of non-vacuum high-temperature brazing; while too little Mg will lead to the formation of Mg 2 Insufficient Si phase makes aluminum alloy material easy to be corroded, which also has an adverse effect on the welding quality of high temperature brazing and reduces the mechanical properties of the material. Therefore, the amount of Mg element can be 0.1%, 0.13%, 0.16%, 0.21%, 0.25%, 0.28%, 0.30%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0041] In some embodiments, the mass ratio of Si to Mg in the aluminum alloy needs to be further controlled. The control of these two elements is also to ensure the formation of sufficient Mg. 2 Si phase, if the mass ratio of Si to Mg is too large, it means that the amount of Si element is too much, which will lead to an increase in the amount of elemental silicon in the alloy material. Once the amount of elemental silicon increases, it will reduce the mechanical properties of the aluminum alloy material. If the mass ratio of Si to Mg is too low, it means that the amount of Mg element in the system is too much, which will lead to Mg 2 If the amount of Si phase formed is insufficient, the tensile strength and yield strength of the aluminum alloy material will also be significantly reduced. Therefore, the mass ratio of Si to Mg can be 2:3, 1.6:1, 2.1:1, 2.0:1, 2.2:1, 6:1, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0042] In some embodiments, the amount of Sr element is controlled at 0.006-0.02%. The addition of Sr element can inhibit the hydrogen absorption of aluminum alloy materials. Hydrogen atoms will dissolve and precipitate during the smelting process of aluminum alloy. During the smelting process of aluminum alloy, hydrogen (H2) will dissolve in the high-temperature aluminum melt. The solubility of hydrogen increases with the increase of temperature. When the molten aluminum alloy cools and solidifies, the solubility of hydrogen drops sharply, because the solubility of hydrogen in solid aluminum alloy is much lower than that in liquid. This process will have a great impact on the mechanical properties, casting properties and heat treatment properties of aluminum alloys: in terms of mechanical properties, the formation of hydrogen bubbles will reduce the strength and plasticity of aluminum alloys, because they will become the location of stress concentration and easily cause cracks; hydrogen will also cause hydrogen embrittlement, especially in high-strength aluminum alloys, hydrogen atoms gather on dislocation lines, reduce the sliding ability, and thus cause the aluminum alloy material to become embrittled; in terms of casting properties, the pores caused by hydrogen will seriously affect the density of aluminum alloy castings, resulting in a decrease in the mechanical properties of the castings, such as tensile strength, fatigue strength and air tightness; in terms of heat treatment properties, aluminum alloys containing a large amount of hydrogen may produce pores during the heat treatment process, affecting the heat treatment effect and the final performance of the material. The present invention suppresses the hydrogen absorption effect by adding trace elements Sr. If the amount of Sr element is too low or not added or the amount is too much, it will affect the inhibitory effect of Sr element on the hydrogen absorption of aluminum alloy materials, resulting in the aluminum alloy material being very easy to form pores and pinholes during the die casting process, reducing the mechanical properties of the aluminum alloy material and affecting the brazing welding quality. Therefore, the amount of Sr can be 0.006%, 0.008%, 0.012%, 0.015%, 0.017%, 0.018%, 0.020%, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.

[0043] In some embodiments, the present invention studies rare earth elements when selecting raw materials. Although Ce and La can both play a role in grain refinement, their effects on the casting properties of the aluminum alloy material described in the present invention are completely different: Ce can improve the fluidity of the aluminum alloy, reduce the formation of shrinkage cavities and pores, and improve the density and surface quality of the casting; but La improves the high-temperature strength and creep performance of the aluminum alloy, causing its casting performance to decline, and the strengthening phase formed by La and Al is not as stable as the strengthening phase formed by Ce and Al, so the present invention chooses to add the Ce element. The Ce element can significantly improve the structure and properties of the aluminum alloy described in the present invention, so that it forms an AlFeSiCe phase with Fe and Si. This phase can effectively refine the grains of the aluminum alloy. This is because Ce atoms act as heterogeneous nucleation centers during the solidification process and can promote the formation of finer grains; at the same time, some Ce elements can also form a strengthening phase CeAl with Al elements. 3, the strengthening phase can be evenly distributed in the aluminum alloy material, significantly improving the hardness and strength of the aluminum alloy material. In the aluminum alloy material system of the present invention, when the Ce element dosage is too low, the amount of Ce element in the system will be too small, insufficient to form AlFeSiCe phase with Fe and Si, which will make the grain size of the alloy larger and difficult to reduce the thermal cracking tendency of the alloy, resulting in insufficient mechanical properties of the solder joint after brazing. When Ce is excessive, the excessive Ce element will form AlCe phase with Al, and the formation of this phase will cause the degree of distortion of the aluminum alloy material structure to increase, so that the mechanical properties of the aluminum alloy material are reduced. Therefore, the dosage of Ce rare earth element can be 0.3%, 0.31%, 0.38%, 0.41%, 0.53%, 0.68%, 0.73%, 0.85%, 0.94%, 1.0%, etc., as well as all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0044] In some embodiments, the melting point of the aluminum alloy is 640-655°C, which can be 640°C, 645°C, 648°C, 650°C, 655°C, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0045] In some embodiments, the thermal conductivity of the aluminum alloy is 180-215 W / mK, which can be 180 W / mK, 182 W / mK, 185 W / mK, 188 W / mK, 201 W / mK, 205 W / mK, 215 W / mK, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.

[0046] In some embodiments, the aluminum alloy has a tensile strength greater than 120 MPa, a yield strength greater than 60 MPa, and an elongation greater than 8%.

[0047] 2. A method for preparing a high thermal conductivity die-casting high temperature brazing aluminum alloy

[0048] Step 1: preparing materials so that the proportion of each component meets the requirements of the aluminum alloy of the present invention; wherein the raw materials include aluminum ingots, magnesium ingots, iron additives, industrial silicon, aluminum strontium alloy, and aluminum cerium alloy;

[0049] Step 2: Place the aluminum ingot in a melting furnace and heat it to melt to obtain aluminum liquid. The temperature of the aluminum liquid is controlled at 730-780°C. Then, industrial silicon and iron additives are added. After all are melted, the temperature is lowered to 700-730°C, and a refining agent is added to refine the aluminum liquid.

[0050] Step 3: Add magnesium ingot and aluminum-cerium alloy to the aluminum liquid obtained in step 2, control the temperature at 680-700°C after all are melted, add aluminum-strontium alloy, detect its components after all are melted, perform degassing after qualified, and maintain the aluminum liquid temperature at 680-700°C;

[0051] Step 4: The aluminum liquid obtained in step 3 is hydraulically pressed into the mold for die casting, and the obtained casting is subjected to aging treatment to obtain the high thermal conductivity die-cast high-temperature brazing aluminum alloy. The die-casting mold temperature controller is pre-maintained at 260-300°C. At the same time, the die-casting mold is equipped with an insulation barrel. During die casting, the barrel temperature is maintained at 280-350°C. The aluminum liquid is cast at a pressure of 65-75MPa. The vacuum degree of the mold cavity of the die-casting machine is below 5KPa. The injection speed is 4-5m / s to quickly enter the die-casting mold, and the die-casting aluminum alloy casting is obtained by cooling and molding. Aging treatment process of casting products: aging temperature: 250-350°C; aging insulation time: 3-4 hours.

[0052] In the preparation method of the present invention, the steps of the preparation method need to be strictly controlled:

[0053] (1) The final temperature of the aluminum liquid before die casting needs to be strictly controlled. If the temperature is too high, the metamorphic and strengthening elements are easily burned, and the hydrogen absorption rate of the alloy aluminum liquid increases. The number of pinholes after die casting is likely to increase, which will reduce the strength and thermal conductivity of the alloy material. If the aluminum liquid temperature is too low, it is easy to affect the fluidity of the die-casting alloy. The aluminum liquid temperature needs to be controlled within the range described in the present invention.

[0054] (2) The aging temperature needs to be strictly controlled. If the temperature is too high, thin-walled parts are prone to high-temperature deformation. If the temperature is too low, aging precipitation and aging strengthening are insufficient, affecting the thermal conductivity and mechanical properties, and failing to improve the thermal conductivity and mechanical properties. The deformation of the parts will reduce the quality of the brazing weld.

[0055] 3. Application of a high thermal conductivity die-casting high temperature brazing aluminum alloy

[0056] The above aluminum alloy or the aluminum alloy prepared by the above preparation method is used to prepare a heat dissipation temperature control liquid cooling module assembly through brazing. The specific steps are as follows:

[0057] Step ①: using the high thermal conductivity die-casting high temperature brazing aluminum alloy of the present invention as a raw material, and die-casting aluminum alloy parts using the above steps and methods;

[0058] Step ②: Remove the riser of the die-cast aluminum alloy parts; remove burrs; perform aging heat treatment; and machine the parts;

[0059] Step 3: Degrease the brazed parts; spray fiber; dry; assemble and fix;

[0060] Step ④: In a high-purity nitrogen atmosphere; perform continuous tunnel furnace brazing; the high-temperature brazing temperature range is 590-610℃;

[0061] Step ⑤: Laser marking;

[0062] Step ⑥: Helium air tightness check;

[0063] Step 7: Component size inspection;

[0064] Step ⑧: Finished product packaging; obtaining a high thermal conductivity die-cast high temperature brazing aluminum alloy heat dissipation temperature control liquid cooling module assembly.

[0065] 4. Examples and Comparative Examples

[0066] Table 1 (Unit: wt%)

[0067]

[0068] Embodiment 1:

[0069] Step 1: Weigh the raw materials according to the proportion of each element in Table 1. The raw materials are weighed according to the composition of the high thermal conductivity die-casting high temperature brazing die-casting aluminum alloy, and the raw materials include aluminum ingots, magnesium ingots, iron additives, industrial silicon, aluminum strontium alloy, and aluminum cerium alloy;

[0070] Step 2: Place the aluminum ingot in a melting furnace and heat it to melt to obtain aluminum liquid. The temperature of the aluminum liquid is controlled at 730-780°C. Then, industrial silicon and iron additives are added. After all are melted, the temperature is lowered to 700-730°C, and a refining agent is added to refine the aluminum liquid.

[0071] Step 3: Add magnesium ingot and aluminum-cerium alloy to the aluminum liquid obtained in step 2, control the temperature at 680-700°C after all are melted, add aluminum-strontium alloy, detect its components after all are melted, perform degassing after qualified, and maintain the aluminum liquid temperature at 680-700°C;

[0072] Step 4: The aluminum obtained in step 3 is hydraulically pressed into a mold for die casting, and the obtained casting is subjected to aging treatment to obtain the high thermal conductivity and high temperature brazing die casting aluminum alloy casting product.

[0073] Step 4: Obtain an aluminum alloy solution in an insulated state, and then use a robot to press the aluminum alloy hydraulically into the die-casting mold cavity to obtain a die-cast aluminum alloy casting.

[0074] Step 5: The die casting mold temperature controller is pre-maintained at 260-300°C. At the same time, the die casting mold is equipped with an insulation barrel. During die casting, the barrel temperature is maintained at 280-350°C. The aluminum liquid is cast at a pressure of 65-75MPa. The vacuum degree of the mold cavity of the die casting machine is below 5KPa. The injection speed is 4-5m / s to quickly enter the die casting mold, and the die casting aluminum alloy casting is obtained by cooling.

[0075] Step 6: Aging treatment: The die castings with the risers removed are subjected to artificial aging treatment. Aging treatment process: Aging temperature: 250-350°C; Aging insulation time: 3-4 hours.

[0076] Step 7: Process the die casting obtained after step 6 into a high thermal conductivity die-cast high temperature brazing aluminum alloy heat dissipation temperature control liquid cooling module assembly.

[0077] The embodiments and comparative examples adopt the component ratios of Table 1, and the preparation method of Example 1 is adopted to prepare high thermal conductivity die-cast high temperature brazing aluminum alloy heat dissipation temperature control liquid cooling module assemblies, and these module assemblies are subjected to tensile tests and thermal conductivity tests. These module assemblies are subjected to room temperature mechanical property tests and thermal conductivity tests: according to GB / T 228.1-2021 Metallic Materials Tensile Test Part 1: Room Temperature Test Method Test; Thermal conductivity is measured according to ASTM-E1461 Flash Method for Determining Fixed Thermal Conductivity Standard Test Method.

[0078] Table 2

[0079] Test Parameters Tensile strength(MPa) Yield strength(MPa) Elongation(%) Thermal conductivity (W / mk) Example 1 124 64 12.1 205 Example 2 128 68 11.9 201 Example 3 133 73 11.2 188 Example 4 139 78 10.5 185 Example 5 143 84 8.8 182 Comparative Example 1 114 59 12.4 206 Comparative Example 2 109 56 12.2 202 Comparative Example 3 139 77 6.8 170 Comparative Example 4 100 56 20 186 Comparative Example 5 116 55 7.8 178 Comparative Example 6 95 54 5.1 158 Comparative Example 7 113 53 6.9 168 Comparative Example 8 108 52 6.4 165

[0080] Combining Table 1 and Table 2, we can see that:

[0081] (1) The results show that the die-cast high-temperature brazing aluminum alloys prepared by the element content and composition of the present invention have excellent mechanical properties and thermal conductivity. Examples 1 to 5 can meet the requirements of tensile strength, yield strength, elongation and thermal conductivity: tensile strength>120MPa, yield strength>60MPa, elongation>8%; thermal conductivity: 180-215W / mK. At the same time, when the aluminum alloy die-castings in Examples 1 to 5 are brazed at high temperature, the die-casting body does not melt, ensuring that the brazing quality can meet the requirements; and the brazing seams obtained after brazing the parts with these materials are full, and the mechanical properties of the welds are high, which can meet the requirements.

[0082] (2) Compared with Example 1, the Si element in Comparative Example 1 exceeds the required element range, and the amount of Si element is reduced, resulting in weakened fluidity of the alloy material and the alloy strengthening phase Mg 2 The content of Si phase is relatively reduced, which eventually leads to the weakening of the tensile mechanical properties of the material.

[0083] (3) Compared with Example 2, the Mg element in Comparative Example 2 exceeds the set element range, and the amount of Mg element is reduced, resulting in a reduction in the strengthening elements of the alloy material. The alloy strengthening phase Mg formed in the material 2 The relative reduction of Si phase causes the weakening of the tensile mechanical properties of the material.

[0084] (4) Compared with Example 3, in Comparative Example 3, the Fe element content is too high, resulting in an excessive number of AlFe phases formed in the alloy, and these AlFe phases basically maintain a needle-like morphology and grow into a needle-like structure of a certain length, causing the material to have a decreased elongation and thermal conductivity. In Comparative Example 4, the Fe element content is too low, resulting in an excessive number of AlFe phases in the alloy phase, and the tensile strength and yield strength of the aluminum alloy material are reduced, while the elongation and thermal conductivity are increased. Moreover, the alloy material of Comparative Example 4 adheres to the die during the die-casting process, and the die-casting yield rate is reduced.

[0085] (5) Compared with Example 4, in Comparative Example 5, the Sr element is too little, so that the Si in the alloy does not undergo deterioration, and the original strengthening element Si in the alloy is not sufficiently deteriorated, which makes the alloying of the obtained material insufficient, reducing the mechanical properties and thermal conductivity of the material; at the same time, the aluminum alloy material prepared in Comparative Example 5 has a serious hydrogen absorption phenomenon, and a large number of hydrogen bubbles are formed in the aluminum alloy material, and are distributed at the position of stress concentration, making the material easy to cause cracks during the die casting process. In Comparative Example 6, the Sr element is too much, so that the aluminum alloy material undergoes excessive qualitative changes, but weakens the deterioration effect. At the same time, the metal structure of the aluminum alloy material in Comparative Example 6 also has a serious hydrogen absorption phenomenon, and the gas content of the structure increases, which reduces the mechanical properties and thermal conductivity of the material.

[0086] (6) Compared with Example 5, in Comparative Example 7, the Ce element content is insufficient, the amount of Ce element is lower than the range value, the effect of Ce element in refining α-Al grains is significantly weakened, the AlFe phase basically maintains a needle-like morphology, and grows into a needle-like structure of a certain length; resulting in a decrease in the tensile strength, yield strength, elongation and thermal conductivity of the material. In Comparative Example 8, the Ce element content is excessive, the amount of Ce element is higher than the range value, the effect of Ce element in refining α-Al grains is significantly weakened, the AlFe phase basically maintains a needle-like morphology, and grows into a needle-like structure of a certain length; resulting in a decrease in the tensile strength, yield strength, elongation and thermal conductivity of the material.

[0087] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.

Claims

1. A high thermal conductivity die-cast high temperature brazing aluminum alloy, characterized in that: Calculated by mass percentage, the aluminum alloy includes the following components: Si is 0.2-0.6%, Fe is 0.8-1.5%, Ce is 0.3-1.0%, Mg is 0.1-0.3%, Sr is 0.006-0.02%; The remaining elements are all impurity elements, and the content of a single impurity element is less than 0.05%, the total amount of the impurity elements is less than 0.15%, and the balance is aluminum.

2. The high thermal conductivity die-cast high temperature brazing aluminum alloy according to claim 1, characterized in that: In the aluminum alloy, the mass ratio of Si to Mg is (2-18):

3.

3. The high thermal conductivity die-cast high temperature brazing aluminum alloy according to claim 1, characterized in that: The melting point of the aluminum alloy is 640-655°C.

4. The high thermal conductivity die-cast high temperature brazing aluminum alloy according to claim 1, characterized in that: The thermal conductivity of the aluminum alloy is 180-215 W / mK.

5. The high thermal conductivity die-cast high temperature brazing aluminum alloy according to claim 1, characterized in that: The aluminum alloy has a tensile strength greater than 120 MPa, a yield strength greater than 60 MPa, and an elongation greater than 8%.

6. A method for preparing a high thermal conductivity die-cast high temperature brazing aluminum alloy, characterized in that: The aluminum alloy according to any one of claims 1 to 5 is prepared by the following specific steps: Step 1: preparing materials so that the proportion of each component satisfies the aluminum alloy of claim 1; wherein the raw materials include aluminum ingots, magnesium ingots, iron additives, industrial silicon, aluminum strontium alloy, and aluminum cerium alloy; Step 2: Place the aluminum ingot in a melting furnace and heat it to melt to obtain aluminum liquid. The temperature of the aluminum liquid is controlled at 730-780°C. Then, industrial silicon and iron additives are added. After all are melted, the temperature is lowered to 700-730°C, and a refining agent is added to refine the aluminum liquid. Step 3: Add magnesium ingot and aluminum-cerium alloy to the aluminum liquid obtained in step 2, control the temperature at 680-700°C after all are melted, add aluminum-strontium alloy, detect its components after all are melted, perform degassing after qualified, and maintain the aluminum liquid temperature at 680-700°C; Step 4: The aluminum obtained in step 3 is hydraulically pressed into a mold for die casting, and the obtained casting is subjected to aging treatment to obtain the high thermal conductivity die-cast high temperature brazing aluminum alloy.

7. The preparation method according to claim 6, characterized in that: In step 4, before die-casting, the die-casting mold is kept at a temperature of 260-300° C.; during die-casting, the aluminum liquid is cast in a barrel at 280-350° C. and a pressure of 65-75 MPa.

8. The preparation method according to claim 6, characterized in that: In step 4, the aging treatment process is: aging temperature: 250-350° C.; aging insulation time: 3-4 hours.

9. An application of a high thermal conductivity die-casting high temperature brazing aluminum alloy, characterized in that: A heat dissipation and temperature control liquid cooling module assembly is prepared by brazing the aluminum alloy described in any of claims 1 to 5 or the aluminum alloy prepared by the preparation method described in any of claims 6 to 8.

Citation Information

Cited By

  • Cast aluminum alloy material as well as preparation method and application thereof

    CN120575074A