Heat treatment method for improving biological performance of plasma spraying white phosphorite coating
By annealing the plasma sprayed alkaline coating at a suitable temperature, the problem of reduced crystallinity of the coating is solved, the biological performance and stability are improved, and the service life of the coating is extended, making it suitable for the application of biomedical materials. .
Patent Information
- Application Number
- CN202310360085.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-15
AI Technical Summary
The crystallinity of the plasma-sprayed alkaline coating decreases during the thermal spraying process, which leads to serious consequences such as aseptic loosening and implantation failure after implantation in the human body. It is difficult to effectively improve the mechanical properties and stability of the coating with existing technology. .
The plasma sprayed leucomonite coating is annealed at a suitable temperature (700~850°C) to improve the crystallinity and biological activity of the coating. The leucomonite powder is prepared and deposited by the plasma spraying process, and then in Annealing is performed at a specific temperature and time to eliminate internal stress, form refined grains, and improve the shape and stability of the coating.
It significantly improves the crystallinity and biological properties of the coating, enhances the osseointegration ability of the implant surface, and extends the service life of the coating. The process is simple and the operation is convenient for large-scale production.
Smart Images

Figure CN118773534A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic-based composite materials and the technical field of biomedical materials, and specifically relates to a heat treatment method for improving the biological performance of a plasma-sprayed whiojasite coating. Background Art
[0002] White calcium phosphate (WH: Ca8Mg2(HPO4)2(PO4) 12 ) is the second most abundant inorganic component in human bone minerals. Compared with hydroxyapatite (HAp: Ca 10 (PO4)6(OH)2) is rich in magnesium and has excellent bone-promoting, nerve and blood vessel protective effects.
[0003] The plasma spraying process is a preparation technology for the surface coating of bone implants in the human body approved by the State Food and Drug Administration. It can instantly melt ceramic particles into small droplets, spray and deposit them on the surface of the substrate. The resulting coating is uniform, dense and has high deposition efficiency. The white phosphate coating prepared by the plasma spraying process has excellent biological activity, which can promote osteoblast proliferation and adhesion and accelerate the bone integration process. However, the crystallinity of the WH coating will be reduced during the thermal spraying process, and aseptic loosening is prone to occur after implantation in the human body, which can lead to serious consequences such as implantation failure. Therefore, improving the biological properties of plasma sprayed white phosphate coatings is the key to expanding the application of white phosphate in the field of biomedical materials technology.
[0004] Therefore, there is an urgent need to provide a method with simple process and easy operation, which can improve the mechanical properties of the coating, improve the stability of the coating, and thus extend the service life of the coating. Summary of the invention
[0005] In view of the above problems, the object of the present invention is to provide a heat treatment method for improving the biological properties of a plasma sprayed white calcium phosphate coating, wherein the plasma sprayed white calcium phosphate coating is annealed at a suitable temperature. The method has a simple process and is easy to operate, and the obtained coating has good crystallinity and osteogenic activity.
[0006] The present invention provides a heat treatment method for improving the biological properties of a plasma sprayed whitlockite coating, comprising:
[0007] (1) preparing white calcium phosphate powder;
[0008] (2) depositing the prepared whiojasite powder on the surface of a substrate through a plasma spraying process to obtain the whiojasite coating composition;
[0009] (3) The plasma sprayed white calcium phosphate coating is annealed, wherein the annealing temperature is 700-850° C. and the time is 2-4 hours.
[0010] Preferably, in step (1), the preparation process of the white phosphate calcium stone powder comprises: weighing Ca(OH)2 and Mg(OH)2 in sequence, adding them into deionized water, and stirring at a constant temperature to obtain a raw material solution; then, adding an aqueous solution with a concentration of 0.6-0.7MH3PO4 dropwise into the raw material solution, controlling the molar ratio of Ca(OH)2:Mg(OH)2:H3PO4 to be 7-8:2-3:6-14, preferably 37:13:50; aging the mixed solution at room temperature, discarding the supernatant, centrifuging, and washing to neutrality; drying, grinding, sieving, and drying to obtain the white phosphate calcium stone powder.
[0011] Preferably, the aging time at room temperature is 24 to 36 hours.
[0012] Preferably, the drying temperature is 60-105° C., preferably 90-100° C.; the drying time is 36-72 h, preferably 48-60 h.
[0013] Preferably, the particle size of the white phosphate powder is controlled to be 60 to 300 microns, preferably 80 to 150 microns.
[0014] Preferably, the substrate is pretreated before the plasma spraying process, and the pretreatment process is: sandblasting the substrate, then ultrasonically cleaning it in deionized water or ethanol for 10 to 20 minutes, and drying it in an oven at 60 to 80° C. for 60 to 120 minutes.
[0015] Preferably, in step (2), the substrate is a medical metal or medical alloy material, preferably pure titanium, titanium alloy, stainless steel or cobalt-chromium-molybdenum alloy.
[0016] Preferably, in step (2), the parameters of the plasma spraying process are: plasma gas Ar flow rate 45-55 standard liters / minute; plasma gas H2 flow rate 5-8 standard liters / minute; spraying distance 200-230 mm; spraying power 27-30 kW; powder feeding rate 8.0-30 g / minute; voltage 55-60 V; current 450-530 A.
[0017] Preferably, in step (3), the heating rate of the annealing treatment is 3-10°C / min, and the cooling rate is 10-20°C / min.
[0018] Appropriate heat treatment methods are effective ways to improve the mechanical properties and stability of the coating, thereby extending the service life of the coating. At higher annealing temperatures, the grains are rearranged, eliminating internal stress, and refined grains are formed after recrystallization, which improves the plasticity of the coating and enables slow and uniform degradation. When the degradation rate of the coating matches the bone ingrowth rate, it is more conducive to the bone integration of the implant.
[0019] Beneficial effects:
[0020] The heat treatment method of the present invention not only greatly improves the crystallinity of the coating, but also has good performance in promoting osteocyte adhesion, alkaline phosphatase expression and extracellular matrix mineralization, and can enhance bone integration on the implant surface; and the preparation method of the present invention has the advantages of simple operation, high efficiency, good repeatability, and suitability for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The XRD spectrum of the WH coating of Example 1 obtained by annealing at 800° C. for 3 hours is as follows: Figure 2 This is the XRD pattern of the WH coating obtained in Comparative Example 1 without annealing treatment; Figure 3 Surface and cross-sectional SEM images of the WH coating of Comparative Example 1 and the WH-800 coating of Example 1; Figure 4 Thermogravimetric-differential thermal (TG-DTA) diagram of the white calcium phosphate coating of Comparative Example 1; Figure 5 The XRD spectrum of the WH-200 coating obtained by annealing at 200°C for 3 hours in Comparative Example 2; Figure 6 The XRD spectrum of the WH-400 coating obtained by annealing at 400°C for 3 hours in Comparative Example 3; Figure 7 The XRD spectrum of the coating WH-600 obtained by annealing at 600°C for 3 hours in Comparative Example 4; Figure 8 The XRD spectrum of the coating WH-1000 obtained by annealing the WH coating of comparative example 5 at 1000°C for 3 hours; Fig. 9 The WH coating of comparative example 6 was annealed at 800°C for 1 hour to obtain the XRD spectrum of the coating WH-800#; Fig.10 The XRD spectrum of the coating WH-800* obtained by annealing the WH coating of comparative example 7 at 800°C for 5 hours; Fig.11 is the XRD pattern of the HAp coating of Comparative Example 8; Fig.12 Schematic diagram of the adhesion morphology and spreading area of MC3T3-E1 cells on the HAp coating of Comparative Example 6, the WH coating of Comparative Example 1, and the WH-800 coating of Example 1; Fig.13Schematic diagram of the proliferation of MC3T3-E1 cells on the surfaces of HAp coating, WH coating and WH-800 coating; Fig.14 Alkaline phosphatase activity of MC3T3-E1 cells on the surfaces of HAp coating, WH coating and WH-800 coating; Fig.15 The results of extracellular matrix mineralization of MC3T3-E1 cells on the surfaces of HAp coating, WH coating and WH-800 coating. DETAILED DESCRIPTION
[0022] To further explain the content, features and practical effects of the present invention, the present invention is described in detail below in conjunction with the embodiments. It should be pointed out that the modification method of the design of the present invention is not limited to these specific implementation methods. Without departing from the spirit and connotation of the design of the present invention, the equivalent replacement and modification made by those skilled in the art on the basis of reading the content of the present invention are also within the scope of the present invention.
[0023] Magnesium-rich whitlockite (WH) is the second most abundant inorganic component in human bones after hydroxyapatite. Its chemical formula is Ca 18 Mg2(HPO4)2(PO4) 12 , has excellent osteogenic, nerve and vascular protection effects. The white calcium phosphate coating prepared by plasma spraying technology has excellent biological activity, can promote osteoblast proliferation and adhesion, and accelerate the process of bone integration. However, the crystallinity of the WH coating will be reduced during thermal spraying, and aseptic loosening will easily occur after implantation into the human body, and serious consequences such as implantation failure will occur. Suitable heat treatment methods are effective ways to improve the mechanical properties of the coating and improve the stability of the coating, thereby extending the service life of the coating. The heat treatment method used in the present invention to improve the biological properties of plasma sprayed white calcium phosphate coating is to anneal the coating at a suitable temperature. At a suitable annealing temperature, the grains are rearranged, internal stress is eliminated, and refined grains are formed after recrystallization, so that the shaping of the coating is improved, and slow uniform degradation can be achieved. When the degradation rate of the coating matches the bone ingrowth rate, it is more conducive to the bone integration of the implant.
[0024] The following is an exemplary description of the heat treatment method provided by the present invention for improving the biological properties of the plasma sprayed whitlockite coating.
[0025] The chemical precipitation method is used to prepare white calcium phosphate powder. Ca(OH)2 and Mg(OH)2 are weighed and added to deionized water in sequence, and stirred at a constant temperature to obtain a raw material solution; then, a 0.6-0.7M H3PO4 aqueous solution is added dropwise to the raw material solution, and the molar ratio of Ca(OH)2:Mg(OH)2:H3PO4 is controlled to be 7-8:2-3:6-14, preferably 37:13:50; the mixed solution is aged at room temperature, the supernatant is discarded, centrifuged, and washed to neutrality; dried, ground, sieved, and dried to obtain the white calcium phosphate powder.
[0026] In an optional embodiment, the aging time at room temperature is 24 to 36 hours.
[0027] The drying temperature is 60-105° C., preferably 90-100° C.; the drying time is 36-72 hours, preferably 48-60 hours.
[0028] The particle size of the white calcium phosphate powder is controlled to be 60 to 300 microns, preferably 80 to 150 microns.
[0029] The prepared whilapite powder is deposited on the surface of the substrate through a plasma spraying process to obtain the whilapite coating composition.
[0030] In an optional embodiment, the substrate is pretreated before the plasma spraying process, and the pretreatment process is: sandblasting the substrate, then ultrasonically cleaning it in deionized water or ethanol for 10 to 20 minutes, and drying it in an oven at 60 to 80° C. for 60 to 120 minutes.
[0031] The substrate is a medical metal or medical alloy material, preferably pure titanium, titanium alloy, stainless steel or cobalt-chromium-molybdenum alloy.
[0032] The parameters of the plasma spraying process are: plasma gas Ar flow rate 45-55 standard liters / minute; plasma gas H2 flow rate 5-8 standard liters / minute; spraying distance 200-230 mm; spraying power 27-30 kilowatts; powder feeding rate 8.0-30 grams / minute; voltage 55-60V; current 450-530A.
[0033] Annealing treatment of plasma sprayed whitlockite coating.
[0034] In an optional embodiment, the annealing temperature is 700-850°C. If the annealing temperature is too low, the crystallinity of the coating cannot be effectively improved, and there will be impurity phases. If the annealing temperature is too high, the coating will melt, and the surface material will be lost and decomposed. The annealing time is 2-4h. If the annealing time is too short, the coating cannot be completely crystallized. If the annealing time is too long, it will not affect the coating performance, but there will be a waste of resources and time. The heating rate of the annealing treatment is 3-10°C / min, and the cooling rate is 10-20°C / min.
[0035] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0036] Example 1
[0037] (1) Preparation of white phosphate coating (WH) by plasma spraying process. 13.71g of Ca(OH)2 and 3.79g of Mg(OH)2 were added to 500mL of deionized water at 80°C in sequence, and stirred at constant temperature for 1 hour to obtain a raw material solution; 20.5mL of H3PO4 with a volume fraction of 85% was dissolved in 500mL of deionized water to obtain an H3PO4 aqueous solution, and the H3PO4 aqueous solution was slowly added dropwise to the above raw material solution; aged at room temperature for 24h, the supernatant was discarded, centrifuged, washed to neutrality, and dried in an oven at 100°C for 48h. The agglomerated powder after drying was ground and passed through 100 and 200 mesh sieves, and the powder between the two sieves was taken and dried to finally obtain white phosphate powder with a particle size of 60 to 100 microns. After the Ti-6Al-4V alloy surface was sandblasted (pressure 0.3MPa), it was ultrasonically cleaned in anhydrous ethanol solution for 15 minutes, and then dried in an oven at 80°C for 1 hour for use. The prepared white calcium phosphate powder was sprayed onto the pretreated titanium alloy surface using a plasma spraying process to obtain a WH coating composition. The plasma spraying process parameters are as follows: the plasma gas Ar flow rate is 50slpm (standard liters / minute), the plasma gas H2 flow rate is 5slpm, the spraying distance is 220mm, the spraying power is 28.5kW, the powder feeding rate is 10g / min; the voltage is 57.8V, and the current is 500A.
[0038] (2) Annealing the plasma sprayed white calcium phosphate coating. The obtained white calcium phosphate coating was placed in an alumina crucible and placed in a muffle furnace. The annealing temperature was set to 800°C, the annealing time was 3h, the heating rate was 5°C / min, and the cooling rate was 15°C / min. After cooling to room temperature, the coating was taken out to obtain the annealed sample WH-800 coating.
[0039] Figure 1 The XRD spectrum of the WH-800 coating obtained by annealing the WH coating of Example 1 at 800°C for 3 hours is shown in the figure. As can be seen from the figure, the phases of the WH-800 coating after annealing at 800°C are white apatite and a small amount of calcium phosphate, and the spectrum peak is sharp, indicating that the crystallinity of the coating is good.
[0040] Comparative Example 1
[0041] The process of preparing the white phosphate coating by plasma spraying process in this comparative example 1 refers to that in Example 1, except that the obtained WH coating is not subjected to the annealing process of step (2).
[0042] Figure 2 This is the XRD spectrum of the WH coating prepared by annealing treatment in Comparative Example 1. As can be seen from the figure, the XRD spectrum peak of the WH coating has a large bun peak, indicating that the crystallinity of the coating is not high.
[0043] Figure 3 The SEM images of the WH coating prepared in Comparative Example 1 and the WH-800 coating prepared in Example 1 are shown. As can be seen from the figure, the surface of the WH coating is a typical semi-molten state morphology obtained by plasma spraying, while the surface of the WH-800 coating can clearly distinguish the close stacking of grains, indicating that the layered structure of the WH-800 coating is denser than that of the WH coating.
[0044] Figure 4 The thermogravimetric-differential thermal (TG-DTA) diagram of the white calcium phosphate coating of comparative example 1. It can be seen from the figure that the coating has obvious exothermic peaks at 93.39°C, 551.44°C and 695.27°C, respectively, which means that the coating will crystallize, oxidize or solidify at these three temperatures. Therefore, the effect of different annealing temperatures on the coating composition and crystallinity can be studied.
[0045] Comparative Example 2
[0046] The process of preparing the white calcium phosphate coating by plasma spraying process in this comparative example 2 refers to Example 1, with the only difference that the annealing temperature in step (2) is 200°C, and the other annealing parameters are referred to Example 1, to obtain the annealed sample WH-200 coating.
[0047] Comparative Example 3
[0048] The process of preparing the white calcium phosphate coating by plasma spraying process in this comparative example 3 refers to that in Example 1, the only difference is that the annealing temperature in step (2) is 400° C., and the other annealing parameters are the same as those in Example 1, to obtain the annealed sample WH-400 coating.
[0049] Comparative Example 4
[0050] The process of preparing the white calcium phosphate coating by plasma spraying process in this comparative example 4 refers to that in Example 1, the only difference is that the annealing temperature in step (2) is 600° C., and the other annealing parameters are the same as those in Example 1, to obtain the annealed sample WH-600 coating.
[0051] Comparative Example 5
[0052] The process of preparing the white calcium phosphate coating by plasma spraying process in this comparative example 5 refers to that in Example 1, the only difference is that the annealing temperature in step (2) is 1000° C., and the other annealing parameters are the same as those in Example 1, to obtain the annealed sample WH-1000 coating.
[0053] Figure 5 , 6 , 7, and 8 are the XRD spectra of WH-200, WH-400, WH-600, and WH-1000 obtained by annealing the WH coating at 200℃, 400℃, 600℃, and 1000℃, respectively. Figure 5 It can be seen that the phase composition of WH-200 coating is white phosphate and calcium phosphate; Figure 6 and 7 It can be seen that the physical composition of WH-400 and WH-600 coatings is mainly white calcium apatite and calcium phosphate, and a small amount of hydroxyapatite; Figure 8 It can be seen that the phase composition of the WH-1000 coating is calcium phosphate, which means that the coating has undergone phase decomposition after annealing at this temperature, that is, white calcium apatite has decomposed into calcium phosphate, and the diffraction peak intensity of the matrix has increased significantly, indicating that the coating has melted, resulting in a significant decrease in thickness during resolidification. It can be seen that the higher the annealing temperature, the higher the crystallinity of the coating sample will increase with the increase of the annealing temperature within a certain temperature range, but at too high an annealing temperature, the coating itself will melt at high temperature and fail, and this failure includes the morphology and phase composition of the coating. Therefore, choosing a suitable annealing temperature can effectively improve the crystallinity of the coating.
[0054] Comparative Example 6
[0055] The process of preparing the white calcium phosphate coating by plasma spraying process in this comparative example 6 refers to that in Example 1, the only difference is that the annealing time in step (2) is 1 hour, and the other annealing parameters are the same as in Example 1, to obtain the annealed sample WH-800# coating.
[0056] Fig. 9 The WH coating of comparative example 6 was annealed at 800°C for 1 hour to obtain the XRD spectrum of the coating WH-800#. It can be seen from the figure that although the phase composition of WH-800# is consistent with that of WH-800, its crystallinity is obviously insufficient compared with that of WH-800.
[0057] Comparative Example 7
[0058] The process of preparing the white calcium phosphate coating by plasma spraying process in this comparative example 7 refers to that in Example 1, with the only difference that the annealing time in step (2) is 5 hours, and the other annealing parameters are the same as in Example 1, to obtain the annealed sample WH-800* coating.
[0059] Fig.10 The XRD spectrum of the WH coating of comparative example 7, which was annealed at 800°C for 5 hours, obtained a coating WH-800*. It can be seen from the figure that the phase of WH-800* has not changed significantly, is consistent with WH-800, and has little difference in crystallinity.
[0060] Comparative Example 8
[0061] Hydroxyapatite (HAp) coating was prepared by plasma spraying process. The HAp powder used was purchased from SulzerMetco in Switzerland, and the powder particle size was 15 to 50 microns. After the surface of the Ti-6Al-4V alloy was sandblasted (pressure 0.3MPa), it was ultrasonicated in anhydrous ethanol solution for 15 minutes, and then dried in an oven at 80°C for 1 hour for use. Commercial hydroxyapatite powder was sprayed onto the pretreated titanium alloy surface using a plasma spraying process to obtain a HAp ceramic coating. Among them, the plasma spraying process parameters are as follows: the plasma gas Ar flow rate is 50slpm, the plasma gas H2 flow rate is 8slpm, the spraying distance is 250mm, the spraying power is 32.9kW, the voltage is 59.8V, and the current is 550A.
[0062] Fig.11 This is the XRD spectrum of the HAp coating of Comparative Example 8. As can be seen from the figure, the HAp coating is a pure phase hydroxyapatite with good crystallinity.
[0063] The crystallinity of different coatings of Example 1 and Comparative Examples 1-8 is shown in Table 1. It can be seen from the table that the crystallinity of the WH coating without annealing is only 62.7%. After heat treatment for the same annealing time, as the annealing temperature is increased, the crystallinity of the corresponding WH-200, WH-400, WH-600 and WH-800 coating samples increases successively, which are 65.6%, 70.3%, 73.4% and 87.4% respectively. However, the higher the annealing temperature, the better. When annealing at 1000°C, the crystallinity of the sample WH-1000 coating does not continue to increase, but decreases to a certain extent to 85.7%. This is because the coating has melted at this temperature, recrystallized during the cooling process, and more amorphous phases appeared again; and from the results of XRD phase analysis, it can be seen that the coating has been decomposed in large quantities at this time, and the original white calcium apatite is decomposed into a new phase, namely calcium phosphate, which is something we do not want to happen. Reducing the annealing time, for example, the WH-800# coating obtained by annealing for 1h cannot guarantee the effective improvement of crystallinity to a certain extent; while too long annealing time has no significant effect on the crystallinity of the coating, such as the crystallinity of the WH-800* coating obtained by annealing for 5h is almost the same as that of WH-800 (3h). Therefore, the annealing temperature and time we selected ensure the effective improvement of the crystallinity of the coating under the premise of energy saving and environmental protection.
[0064] Table 1:
[0065] The present invention uses mouse preosteoblasts MC3T3-E1 to conduct cell adhesion, proliferation, ALP activity and ECM mineralization ability to evaluate the biocompatibility of the coating.
[0066] The HAp, WH and WH-800 coating samples were sterilized at 121 °C and 1.5 MPa and then placed in a 48-well plate with a surface inoculation density of 1 × 10 4 cell / well preosteoblasts. After culturing for 24 hours, the samples were washed three times with PBS. The samples were immersed in glutaraldehyde solution overnight and treated with different concentration gradients of alcohol (30%, 50%, 70%, 90%, 100%). After the samples were dried, the adhesion morphology of cells on the coating surface was observed using FE-SEM.
[0067] Fig.12 Schematic diagram of the adhesion morphology and spreading area of MC3T3-E1 cells on the HAp coating of Comparative Example 8, the WH coating of Comparative Example 1, and the WH-800 coating of Example 1. Fig.12From the adhesion and spreading of cells on the coating surface, it can be seen that compared with HAp coating, the filopodia and lamellipodia of cells on the surface of WH and WH-800 coatings are more developed, and the spreading on the material surface is better.
[0068] The samples were sterilized using a steam sterilizer (121°C, 30 min), and each group of sterile materials was carefully placed in a 48-well cell culture plate. MC3T3-E1 cells in good growth condition were collected, digested and the concentration of the cell suspension was adjusted. 1 mL of cell suspension (10,000 cells / mL) was planted on the surface of the sample. After culturing in a 37°C, 5% CO2 cell culture incubator for 1, 4 and 7 days, the culture medium was discarded. 1 mL of fresh culture medium and 0.1 mL of CCK-8 solution were added to each well. After continuing to culture in a 37°C, 5% CO2 cell culture incubator for 3 hours, the solution in each well was carefully aspirated and added to a 48-well plate. The OD value of each well was measured at 450 nm using an ELISA reader.
[0069] Fig.13 The proliferation of MC3T3-E1 cells on the surfaces of HAp, WH and WH-800 coatings. Fig.13 It can be seen from the cell proliferation that the cell proliferation rate of WH and WH-800 coatings is significantly higher than that of HAp coating. Although the cell proliferation level of WH-800 is not as good as that of WH coating, this may be because cell proliferation mainly depends on the bioactive ions (Ca) produced by the degradation of the coating. 2+ and Mg 2+ ), Table 2 lists the ion release of HAp coating, WH coating and WH-800 coating in deionized water. From the ion dissolution in Table 2 (unit: μg / ml), it can be seen that the ion dissolution rate of WH-800 coating with higher crystallinity is relatively small, but the cell proliferation level is still higher than that of HAp coating with larger dissolution amount, indicating that WH-800 can continuously exert a high ability to promote osteoblast proliferation.
[0070] Table 2:
[0071] Sterilized samples were placed in 48-well plates and cells were plated at a density of 1 × 10 4 / well were inoculated on the coating surface. After 7 and 14 days of culture, 200 μL of PBS solution containing 0.2% Triton X-100 was added to each well, respectively, and lysed on ice for 15 minutes. The lysed suspension was then centrifuged for 5 minutes, the supernatant was collected, and transferred to a 96-well plate. 50 μL of the supernatant was mixed with 150 μL of p-nitrophenyl phosphate and cultured for 10 minutes in the dark. The OD value of the supernatant was determined using an enzyme reader. In addition, the total protein content in the cells was detected using the BCA method, and the alkaline phosphatase activity was expressed in enzyme activity units.
[0072] The sterilized samples were placed in a 48-well plate and the cells were plated at a density of 1×10 4 The cells were inoculated on the coating surface at a density of 1 / well. After 14 and 21 days of culture, the samples were washed twice with PBS and fixed with paraformaldehyde solution for 15 minutes. The OD value of the supernatant at 590 nm was measured with an ELISA reader to evaluate the extracellular matrix mineralization behavior.
[0073] Depend on Fig.14 and Fig.15 It can be seen that the WH-800 coating not only has excellent performance in promoting osteocyte adhesion and proliferation, but also has improved performance in promoting alkaline phosphatase secretion and extracellular matrix mineralization compared with HAp and WH coatings.
[0074] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A heat treatment method for improving the biological properties of plasma sprayed whitlockite coating, characterized in that: include: (1) preparing white calcium phosphate powder; (2) depositing the prepared whiojasite powder on the surface of a substrate through a plasma spraying process to obtain the whiojasite coating composition; (3) The plasma sprayed white calcium phosphate coating is annealed, wherein the annealing temperature is 700-850° C. and the time is 2-4 hours.
2. The heat treatment method for improving the biological properties of plasma sprayed whitlockite coating according to claim 1, characterized in that: In step (1), the preparation process of the white phosphate calcium stone powder includes: weighing Ca(OH)2 and Mg(OH)2 in sequence, adding them into deionized water, and stirring at a constant temperature to obtain a raw material solution; then, adding a 0.6-0.7M H3PO4 aqueous solution dropwise into the raw material solution, controlling the molar ratio of Ca(OH)2:Mg(OH)2:H3PO4 to be 7-8:2-3:6-14, preferably 37:13:50; aging the mixed solution at room temperature, discarding the supernatant, centrifuging, and washing to neutrality; drying, grinding, sieving, and drying to obtain the white phosphate calcium stone powder.
3. The heat treatment method for improving the biological properties of plasma sprayed whitlockite coating according to claim 2, characterized in that: The aging time at room temperature is 24 to 36 hours.
4. The heat treatment method for improving the biological properties of plasma sprayed whitlockite coating according to claim 2 or 3, characterized in that: The drying temperature is 60-105° C., preferably 90-100° C.; the drying time is 36-72 hours, preferably 48-60 hours.
5. The heat treatment method for improving the biological properties of plasma sprayed whitlockite coating according to any one of claims 1 to 4, characterized in that: The particle size of the white calcium phosphate powder is controlled to be 60 to 300 microns, preferably 80 to 150 microns.
6. The heat treatment method for improving the biological properties of plasma sprayed whitlockite coating according to any one of claims 1 to 5, characterized in that: The substrate is pretreated before the plasma spraying process. The pretreatment process is as follows: the substrate is sandblasted, then ultrasonically cleaned in deionized water or ethanol for 10 to 20 minutes, and dried in an oven at 60 to 80° C. for 60 to 120 minutes.
7. The heat treatment method for improving the biological properties of plasma sprayed whitlockite coating according to any one of claims 1 to 6, characterized in that: In step (2), the substrate is a medical metal or medical alloy material, preferably pure titanium, titanium alloy, stainless steel or cobalt-chromium-molybdenum alloy.
8. The heat treatment method for improving the biological properties of plasma sprayed whitlockite coating according to any one of claims 1 to 7, characterized in that: In step (2), the parameters of the plasma spraying process are: plasma gas Ar flow rate 45-55 standard liters / minute; plasma gas H2 flow rate 5-8 standard liters / minute; spraying distance 200-230 mm; spraying power 27-30 kilowatts; powder feeding rate 8.0-30 grams / minute; voltage 55-60V; current 450-530A.
9. The heat treatment method for improving the biological properties of plasma sprayed whitlockite coating according to claims 1-8, characterized in that: In step (3), the heating rate of the annealing treatment is 3 to 10°C / min, and the cooling rate is 10 to 20°C / min.
Citation Information
Patent Citations
Preparation method of calcium-magnesium-silicon multiphase ceramic coating for titanium-based artificial joint handle
CN102302799A
Calcium phosphate ceramic activated surface and preparation method thereof
CN103693995A
Whitlockite coating constructed on surface of calcium phosphatebiological ceramic matrix and preparation method of whitlockite coating
CN107141022A