Sediment prevention piece for vacuum environment
By using anti-sediment parts covered with high water droplet contact angles and high-hardness fluorine coatings in a vacuum environment, the problem of material deposition during the semiconductor manufacturing process is solved, achieving self-cleaning and extending the maintenance cycle, and reducing maintenance costs. .
Patent Information
- Application Number
- CN202310553562.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2023-05-17
- Publication Date
- 2024-10-15
AI Technical Summary
In the semiconductor manufacturing process, process gases or exhaust gases are easily deposited or accumulated in fluid channels, resulting in shortened maintenance cycles and affecting manufacturing costs and schedules.
An anti-sediment component for vacuum environments is used, which includes a main structure and a fluorine coating layer covering the surface of the main structure. The fluorine coating layer has a high water droplet contact angle, hardness and acid corrosion resistance, and covers the surface of the process equipment. Inclined, flat or curved parts to prevent sedimentation and scratching.
It effectively prevents deposition, achieves self-cleaning and easy-to-clean effects, enhances adhesion, avoids peeling, extends the maintenance cycle, and saves maintenance costs and manpower.
Smart Images

Figure CN118773576A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a vacuum component, and in particular to an anti-deposition object used in a vacuum environment. Background Art
[0002] In recent years, due to the continuous and vigorous development of semiconductor technology, technological products have made great strides. In the process of semiconductor chip manufacturing, the chip is usually placed in the process equipment to perform related process operations, and a vacuum pump is used to extract the air or gas in the process equipment to keep the process equipment in a negative pressure state, that is, to a certain degree of vacuum. However, in the semiconductor process, process materials such as process gas or process exhaust gas are easily deposited or accumulated in the fluid channel, which leads to shorter and shorter maintenance cycles, thereby affecting the manufacturing cost and schedule. Summary of the invention
[0003] In view of this, one or more objectives of the present invention is to provide an anti-deposition object for use in a vacuum environment to solve the above-mentioned problems of the conventional technology.
[0004] To achieve the aforementioned purpose, the present invention proposes an anti-deposition object for use in a vacuum environment, comprising: a main structure having at least one surface; and a fluorine coating layer covering the surface of the main structure, wherein the anti-deposition object contacts a process material used or discharged by a process equipment in a vacuum environment when performing a process, and the fluorine coating layer has a higher water droplet contact angle with the process material than the surface of the main structure, the fluorine coating layer has a hardness similar to or higher than the surface of the main structure, and the fluorine coating layer has a lower roughness than the surface of the main structure.
[0005] The main structure is an outlet pipe of the process equipment or a pipe or component of a peripheral device of the process equipment.
[0006] The fluorine coating layer is located on the surface of a portion of the main structure, and the portion is an inclined portion, a plane portion or a curved portion of the main structure.
[0007] The fluorine coating layer has a higher acid corrosion resistance and a higher plasma etching resistance than the surface of the main structure.
[0008] The surface of the main structure is roughened to form a rough surface with a rough structure, so as to increase the surface roughness.
[0009] The surface of the main structure is treated by pickling or sandblasting to increase the surface roughness.
[0010] The fluorine coating layer is composed of 0.01-20%wt of fluorocarbons, 5-50wt% of alkoxysilanes, 0.01%-20%wt of catalytic additives and 10-90wt% of solvents.
[0011] The fluorocarbon compound is selected from the group consisting of perfluoroalkane (PFAS), chlorofluorocarbon (CFC), semifluoroalkane (HFC), fluoropolymer (PTFE) and hydrochlorofluorocarbon (HCFC). The main materials are organic / inorganic polymer copolymers of fluorine, nano-titanium, silicon, and silicon elastomer.
[0012] The fluorocarbon compound is a fluorine-containing monomer or polymer containing 1 to 20 carbon atoms.
[0013] The alkoxysilanes are selected from the group consisting of alkoxysilane oligomers, alkoxysilane compounds, alkoxysilane polymers, alkoxysiloxane oligomers, alkoxysiloxane compounds, alkoxysiloxane polymers, alkoxysilazane oligomers, alkoxysiloxane compounds, alkoxysiloxane polymers, alkoxysilazane oligomers, alkoxysilazane compounds and alkoxysiloxane polymers.
[0014] The catalytic additive is selected from the group consisting of metals, metal oxides, phosphates and carboxylates of platinum, titanium, tin, zinc, aluminum, silver, calcium, magnesium, potassium, sodium, nickel, chromium, molybdenum, vanadium, copper, iron, cobalt, germanium, hafnium, lanthanum, lead, ruthenium, tantalum, tungsten and zirconium.
[0015] The solvent is selected from the group consisting of alcohols, ketones, esters, fluoroalcohols, fluoroethers and ethers.
[0016] The alkoxysilane has a reactive functional group, and the reactive group undergoes a self-condensation reaction at room temperature for 1 to 7 days or at a temperature of 40 to 60 degrees Celsius for 1 to 24 hours.
[0017] The process performed by the process equipment is an atomic layer deposition (ALD) process, and the process material is titanium tetrachloride (TiCl4).
[0018] The process performed by the process equipment is a metal organic chemical vapor deposition (MOCVD) process, and the process material is a process gas or a process waste gas.
[0019] The process performed by the process equipment is an Al-pad process, and the process material is a process gas reactant or a process exhaust gas.
[0020] The water drop contact angle of the fluorine coating layer ranges from 100 degrees to 120 degrees.
[0021] The fluorine coating layer can withstand temperatures up to 600 degrees Celsius.
[0022] The hardness of the fluorine coating layer ranges from 8H to 9H.
[0023] The adhesion between the fluorine coating layer and the surface of the main structure is in the range of 4B to 5B according to a hundred-grid test.
[0024] As described above, the anti-deposition object used in a vacuum environment according to the present invention has one or more advantages or technical effects:
[0025] (1) By coating the vacuum components with a high-hardness fluorine coating layer, the vacuum components can be protected from being scratched by particles and other process materials.
[0026] (2) By coating the vacuum parts with a fluorine coating layer with a high water droplet contact angle, deposition on the vacuum parts can be prevented and the effects of self-cleaning and easy cleaning can be achieved.
[0027] (3) The fluorine coating layer has good adhesion to the main structure, which can avoid peeling during the manufacturing process.
[0028] (4) By providing anti-deposition objects with a fluorine coating layer, funds and manpower for frequent maintenance can be saved.
[0029] In order to enable you to have a further understanding and recognition of the technical features and technical effects of the present invention, preferred embodiments and detailed descriptions are provided as follows. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic diagram of the partial structure of the anti-deposition object used in a vacuum environment according to the present invention.
[0031] Figure 2 It is a schematic diagram of the anti-deposition object for vacuum environment of the present invention being applied to process equipment.
[0032] Figure 3It is a schematic cross-sectional structure diagram of a first embodiment of the anti-deposition object used in a vacuum environment of the present invention.
[0033] Figure 4 It is a schematic cross-sectional structure diagram of a second embodiment of the anti-deposition object used in a vacuum environment of the present invention.
[0034] Figure 5 It is a schematic cross-sectional structure diagram of a third embodiment of the anti-deposition object used in a vacuum environment of the present invention.
[0035] Figure 6 It is a schematic diagram of the three-dimensional structure of a fourth embodiment of the anti-deposition object used in a vacuum environment of the present invention.
[0036] Description of reference numerals:
[0037] 10: Anti-deposition objects
[0038] 20: Main structure
[0039] 22: Surface
[0040] 24: Location
[0041] 26: Spiral guide groove
[0042] 30: Fluorine coating layer
[0043] 100: Process equipment
[0044] 110: Process materials
[0045] 120: Rough structure
[0046] θ: water drop contact angle DETAILED DESCRIPTION
[0047] In order to facilitate understanding of the technical features, contents and advantages of the present invention and the effects that can be achieved, the present invention is hereby described in detail in the form of embodiments in conjunction with the drawings. The drawings used therein are only for illustration and auxiliary description purposes, and may not be the actual proportions and precise configurations after the implementation of the present invention. Therefore, the proportions and configurations of the attached drawings should not be interpreted or limited to the scope of rights of the present invention in actual implementation. In addition, for ease of understanding, the same elements in the following embodiments are described with the same symbols.
[0048] In addition, the words used throughout the specification and claims generally have the ordinary meaning of each word used in this field, in the content disclosed herein, and in the specific content, unless otherwise noted. Certain words used to describe the present invention will be discussed below or elsewhere in this specification to provide additional guidance to those skilled in the art in the description of the present invention.
[0049] The use of “first,” “second,” “third,” “fourth,” etc. in this document does not specifically refer to an order or sequence, nor is it used to limit the present invention. It is merely used to distinguish components or operations described with the same technical terms.
[0050] Secondly, the words "include", "including", "have", "contain" and the like used in this article are open terms, which mean including but not limited to.
[0051] See also Figures 1 to 6 , Figure 1 It is a schematic diagram of the partial structure of the anti-deposition object used in a vacuum environment according to the present invention. Figure 2 It is a schematic diagram of the anti-deposition object for vacuum environment of the present invention being applied to process equipment. Figure 3 It is a schematic cross-sectional structure diagram of a first embodiment of the anti-deposition object used in a vacuum environment of the present invention. Figure 4 It is a schematic cross-sectional structure diagram of a second embodiment of the anti-deposition object used in a vacuum environment of the present invention. Figure 5 It is a schematic cross-sectional structure diagram of a third embodiment of the anti-deposition object used in a vacuum environment of the present invention. Figure 6 It is a schematic diagram of the three-dimensional structure of a fourth embodiment of the anti-deposition object used in a vacuum environment of the present invention.
[0052] like Figures 1 to 6 As shown, the anti-deposition object 10 for use in a vacuum environment of the present invention comprises a main structure 20 and a fluorine coating layer 30, wherein the fluorine coating layer 30 covers the main structure 20. The anti-deposition object 10 of the present invention is applied in a vacuum environment, and contacts a process material 110 used or discharged when a process is performed by a process equipment 100 in a vacuum environment, wherein the above-mentioned vacuum environment is not limited to a specific vacuum degree, and it may be determined according to the requirements of the process equipment 100. The fluorine coating layer 30 covers at least one surface 22 of the main structure 20. The fluorine coating layer 30 of the anti-deposition object 10 of the present invention may, for example, cover all or part of the surface of the main structure 20, such as the surface 22 of a portion 24 of the main structure 20. Among them, this portion 24 may be a location where deposition of process materials usually occurs more frequently, such as a non-planar location such as a bend or an inclined location, and for example but not limited to the inner wall surface. Therefore, in the present invention, the above-mentioned portion 24 is, for example, a bend of the main structure 20 (such as Figure 3 as shown) or inclined parts (as shown Figure 4 However, the present invention is not limited thereto. The fluorine coating layer 30 of the present invention can also cover the planar portion of the main structure 20 (such as Figure 5 In addition, the main structure 20 of the anti-deposition object 10 of the present invention is, for example, an outlet pipe of the process equipment 100 (such as Figures 3 to 5) or pipes (such as those of peripheral equipment (such as a vacuum pump) of the process equipment 100 Figures 3 to 5 as shown) or parts (as shown Figure 6 (as shown in the figure) of a Holweck pump part with a spiral guide groove 26. Although the above lists a variety of forms of the main structure 20 of the anti-deposition object 10, the present invention is not limited thereto, and all forms of objects that can be used in a vacuum environment fall within the scope of protection requested by the present invention. For example, the anti-deposition object 10 of the present invention and its main structure 20 may also be, for example, a cavity or component of a vacuum pump, such as the rotor blades and / or stator blades of a turbomolecular vacuum pump (TMP). For example, the anti-deposition object 10 of the present invention and its main structure 20 may also be, for example, a cavity or component of a valve structure. In short, the present invention can selectively form a fluorine coating layer 30 on the surface of all objects that may contact the process material 110.
[0053] One of the characteristics of the anti-deposition object for vacuum environment of the present invention is that the surface 22 of the main structure 20 is covered by the fluorine coating layer 30, so the fluorine coating layer 30 can replace the surface 22 of the main structure 20 to contact the process material 110 used or discharged by the process equipment 100 during the process. The fluorine coating layer 30 can, for example, cover the surface 22 of the main structure 20 by coating, wherein the coating method is for example but not limited to spraying, brushing, dipping or rubbing. The present invention can, for example, directly coat the liquid (fluid state) fluorine coating layer 30 on the surface 22 of the main structure 20, or before coating the liquid fluorine coating layer 30 on the surface 22 of the main structure 20, the surface 22 of the main structure 20 is roughened to increase the surface roughness. The roughening treatment may be, for example, but not limited to, pickling or sandblasting, so as to form a rough surface with more rough structures 120 such as grooves or notches on the surface 22 of the main structure 20, so as to increase the adhesion between the fluorine coating layer 30 and the surface 22 of the main structure 20. The present invention is not limited to specific pickling or sandblasting methods, that is, no matter what technical means are used for the roughening treatment, as long as the surface roughness of the main structure 20 can be increased, it falls within the scope of the protection claimed by the present invention, so it will not be described in detail here.
[0054] After the present invention coats the liquid (fluid state) fluorine coating layer 30 on the surface 22 of the main structure 20, it can be selectively subjected to self-condensation reaction at room temperature for about 1 to 7 days or at a temperature of 40 degrees Celsius to 60 degrees Celsius for about 1 to 24 hours, that is, the fluorine coating layer 30 is cured on the surface 22 of the main structure 20 to form a cured fluorine coating layer 30. The thickness of the fluorine coating layer 30 can range from 1 μm to 3,000 μm, and can be any numerical range or upper and lower limit values within this range, such as from 10 μm to 300 μm. The physical and chemical properties of the fluorine coating layer 30 are better than the original physical and chemical properties of the surface 22 of the main structure 20. For example, in a vacuum environment, the fluorine coating layer 30 has a higher water drop contact angle θ to the process material 110 than the surface 22 of the main structure 20, that is, the water drop contact angle between the fluorine coating layer 30 and the process material 110 (ranging from about 100 degrees to 140 degrees, and can be any numerical range or upper and lower limit values in this range, such as 106.5 degrees) is higher than the water drop contact angle between the surface 22 of the main structure 20 and the process material 110 (ranging from about 89 to 95 degrees). The present invention can prevent the vacuum component from depositing by coating the fluorine coating layer 30 with a high water drop contact angle on the vacuum component, and can achieve the effects of self-cleaning and easy cleaning. The fluorine coating layer 30 has a similar or higher hardness than the surface 22 of the main structure 20, that is, the hardness of the fluorine coating layer 30 (ranging from about 8H to 9H, and can be any numerical interval or upper and lower limit values in this range) is close to, the same as or higher than the hardness of the surface 22 of the main structure 20 (ranging from about 4H to 6.5H). The present invention can prevent the vacuum component from being scratched by the process materials such as particles by coating the high-hardness fluorine coating layer 30 on the vacuum component. The adhesion between the fluorine coating layer 30 and the surface 22 of the main structure 20 (the range of the Cross-Cut test is about 4B to 5B) is higher than the contact force applied by the process material 110 to the fluorine coating layer 30 (e.g., the external force or adsorption force of the process material 110 hitting the fluorine coating layer 30 when it is discharged), so that the fluorine coating layer 30 of the present invention has good adhesion to the main structure 20, which can avoid the peeling phenomenon during the process. The fluorine coating layer 30 has higher acid corrosion resistance and plasma etching resistance than the surface 22 of the main structure 20, so the fluorine coating layer 30 of the present invention can protect the vacuum components from acid corrosion and free radical corrosion. The fluorine coating layer 30 has a lower roughness than the surface 22 of the main structure 20, that is, the roughness of the fluorine coating layer 30 (about 0.2) is lower than the roughness of the surface 22 of the main structure 20, and the fluorine coating layer 30 can even provide the effect of filling or penetrating the rough structure 120 such as grooves or scratches on the surface 22 of the main structure 20, so as to achieve the effect of flattening.In addition, the fluorine coating layer 30 of the present invention can withstand relatively high temperatures, and its operating temperature range is quite wide, and the tolerable temperature can be as high as about 600 degrees Celsius. The operating temperature range of the fluorine coating layer 30 is, for example, less than or equal to about 600 degrees Celsius, preferably, for example, from about 260 degrees Celsius to 600 degrees Celsius, and can be any numerical range or upper and lower limit endpoints less than or equal to 600 degrees Celsius. On the other hand, traditional water-repellent coatings or anti-fouling coatings usually cannot withstand high temperatures, for example, the operating temperature of traditional Teflon is lower than 260 degrees Celsius. Moreover, the hardness of traditional water-repellent coatings or anti-fouling coatings is only about 1H to 3H, for example, the hardness of traditional Teflon is 1H to 2H. It can be seen from this that traditional water-repellent layers or anti-fouling layers cannot withstand the high temperature, high vacuum, high corrosion, high impact and high deposition environment when the process equipment 100 performs semiconductor processes. In other words, the anti-deposition object 10 of the present invention can save money and manpower for frequent maintenance by combining the fluorine coating layer 30 and the main structure 20 .
[0055] The composition of the fluorine coating layer 30 of the present invention may be, for example, composed of fluorocarbons (Fluoro-carbons) accounting for about 0.01% to 20% wt, alkoxysilanes accounting for about 5% to 50% wt, catalytic additives accounting for about 0.01% to 20% wt, and solvents accounting for about 10% to 90% wt. Fluorocarbons are, for example, fluorine-containing monomers or polymers containing 1-20 carbon atoms. For example, fluorocarbons are, for example, fluorine-containing monomers containing about 3 to about 20 carbon atoms and at least one terminal trifluoromethyl group. For example, fluorocarbons are, for example, selected from the group consisting of perfluoroalkanes (PFAS), chlorofluorocarbons (CFCs), semifluoroalkanes (HFCs), fluoropolymers (PTFE) and hydrofluorochlorocarbons (HCFCs). Alkoxysilanes are, for example, selected from the group consisting of alkoxysilane oligomers, alkoxysilane compounds, alkoxysilane polymers, alkoxysiloxane oligomers, alkoxysiloxane compounds, alkoxysiloxane polymers, alkoxysilazane oligomers, alkoxysiloxane compounds, and alkoxysiloxane polymers. The catalytic additive is selected from the group consisting of metals, metal oxides, phosphates and carboxylates of platinum, titanium, tin, zinc, aluminum, silver, calcium, magnesium, potassium, sodium, nickel, chromium, molybdenum, vanadium, copper, iron, cobalt, germanium, hafnium, lanthanum, lead, ruthenium, tantalum, tungsten and zirconium. For example, the catalytic additive is selected from the group consisting of silicon oxide, aluminum oxide, titanium oxide, iron oxide, magnesium oxide, molybdenum oxide, calcium oxide and calcium chloride, and is nano-sized. However, the present invention is not limited to this. Catalytic additives or components of micron-sized or even micron-sized are all within the scope of the present invention. The solvent is, for example, alcohols such as ethanol, propanol or butanol. However, the present invention is not limited to this, and the solvent of the present invention can be selected from the group consisting of alcohols, ketones, esters, fluoroalcohols, fluoroethers and ethers. The alkoxysilanes of the present invention have reactive functional groups, which can undergo self-condensation reaction at room temperature for 1 to 7 days (eg, 7 days) or at 40 to 60 degrees Celsius for 1 to 24 hours (eg, 24 hours).Among them, the above-mentioned reactive functional groups are, for example, hydrosilation reactive functional groups (such as alkenyl, acryloyl, hydrogen atoms bonded to silicon atoms), condensation reactive functional groups (such as hydroxyl, alkoxy, acyloxy) or peroxide curing reactive functional groups (such as alkyl, alkenyl, acryloyl, hydroxyl). In addition, in a feasible implementation, the components of the fluorine coating layer 30 of the present invention can also be, for example, an organic / inorganic polymer copolymer composed of fluorine, nano-titanium, silicon and silicon elastomer. Since those with ordinary knowledge in the technical field to which the present invention belongs should know how to select and modulate the anti-deposition object 10 of the fluorine coating layer 30 having the efficacy of the present invention based on the above content of the present invention, it is not further described here.
[0056] The surface hardness test method of the present invention is to test the surface hardness of the fluorine coating layer 30 with a hardness pencil. For example, a hardness pencil (Mitsubishi standard pencil) is loaded on a fixed load trolley at a 45-degree angle, and then the trolley is pushed by hand to slide over the surface of the fluorine coating layer 30 of the anti-deposition object 10 to confirm the surface hardness when scratched by the pencil. In the anti-deposition object 10 of the present invention, the surface hardness test results of the fluorine coating layer 30 covering the surface 22 of the main structure 20 are all between 8H load 1Kg and 9H load 500g.
[0057] The cross-cut test of the present invention is conducted according to ASTM D3359 method B (cross-cut method), wherein 10×10 (100) 1mm×1mm small grid lines are drawn on the surface of the test sample with a cross-cut knife, and each drawn line should reach the bottom layer of the fluorine coating layer 30 of the anti-deposition object 10; the debris in the test area is cleaned with a brush; a standard tape (3M No. 600 tape) or a tape of equivalent effectiveness is used to stick to the small grid lines to be tested, and the tape is vigorously rubbed with an eraser to increase the contact area and strength between the tape and the test area, and one end of the tape is grasped by hand, and the tape is quickly torn off at an angle of 180 degrees within 1.5 minutes plus or minus 30 seconds, and the peeling state of the fluorine coating layer 30 is observed. In the anti-deposition object 10 of the present invention, the fluorine coating layer 30 of the present invention coated on the surface 22 of the main structure 20 has a hundred-grid test result ranging from 5B (the cut edge is completely smooth, and there is no peeling at the grid edge) to 4B (small pieces peel off at the intersection of the cut, and the actual damage in the grid area is ≤5%). It can be seen that the fluorine coating layer 30 of the present invention has a very high adhesion (closeness) to the surface 22 of the main structure 20.
[0058] The acid corrosion test of the present invention uses 0.05 ml of 5% HCl (hydrochloric acid) to drip on the test sample and let it stand for 24 hours to wait for the HCl solution to evaporate. During the volatilization process, the concentration of HCl in the area will rise and increase the diffusion corrosion effect. After observing the corrosion diffusion area for 24 hours. According to the test results, the corrosion area (mm) of the surface 22 of the main structure 20 without the fluorine coating layer 30 is 2 ) is about 45.13 mm, while the corrosion area (mm) of the surface 22 of the main structure 20 coated with the fluorine coating layer 30 is 2 ) is only about 19.4mm.
[0059] In addition, the present invention has also been subjected to plasma etching tests, and the results show that under the same etching conditions (CHF3:Ar is 1:1, 60 minutes, and the etching rate of oxide is 750nm / 30min), the fluorine coating layer 30 of the present invention does have better plasma etching resistance than the surface 22 (anodized aluminum material) of the main structure 20. As for the thermal stability test (Thermogravimetric Analyzer, TGA test), under the test environment of a heating rate of 5 degrees Celsius / minute and a test atmosphere of N2, the weight of the fluorine coating layer 30 of the present invention shows a stable and slow decrease within the test temperature range (600 degrees Celsius), and no sudden weight change occurs, indicating that the fluorine coating layer 30 of the anti-deposition object 10 of the present invention does not crack.
[0060] The process performed by the process equipment 100 is, for example, a semiconductor process. For example, the process performed by the process equipment 100 is an atomic layer deposition (ALD) process, the process material is titanium tetrachloride (TiCl4), wherein the main structure 20 of the anti-deposition object 10 is, for example, a fluid delivery pipe, but is not limited thereto. For example, the process performed by the process equipment 100 is an organic metal chemical vapor deposition (MOCVD) process, the process material is a process gas or a process exhaust gas, wherein the main structure 20 of the anti-deposition object 10 is, for example, an outlet pipe of a vacuum pump, but is not limited thereto. For example, the process performed by the process equipment 100 is an Al-pad process, and the process material is a process gas reactant or a process exhaust gas, such as selected from the group consisting of N2, O2, Ar, SF6, He, HBr, CF4, CH4, Cl2, BCl3 and CHF3, wherein the main structure 20 of the anti-deposition object 10 is, for example, a pump part with a guide spiral groove and an outlet pipe, but is not limited thereto. The anti-deposition object for vacuum environment of the present invention has been actually tested and has good effects in the above-mentioned processes. For example, in the Al-pad process, the anti-deposition object of the present invention can extend the maintenance cycle by about 20%, thereby reducing the funds and manpower for frequent maintenance.
[0061] In summary, the anti-deposition object for use in a vacuum environment of the present invention has the following advantages:
[0062] (1) By coating the vacuum components with a high-hardness fluorine coating layer, the vacuum components can be protected from being scratched by particles and other process materials.
[0063] (2) By coating the vacuum parts with a fluorine coating layer with a high water droplet contact angle, deposition on the vacuum parts can be prevented and the effects of self-cleaning and easy cleaning can be achieved.
[0064] (3) The fluorine coating layer has good adhesion to the main structure, which can avoid peeling during the manufacturing process.
[0065] (4) By providing anti-deposition objects with a fluorine coating layer, the funds and manpower required for frequent maintenance can be reduced.
[0066] The above description is for illustrative purposes only and is not intended to be limiting. Any equivalent modifications or changes made thereto without departing from the spirit and scope of the present invention shall be included in the appended claims.
Claims
1. An anti-deposition object for use in a vacuum environment, characterized in that: At least: a main structure having at least one surface; and A fluorine coating layer covers the surface of the main structure, wherein the anti-deposition object contacts a process material used or discharged by a process equipment in a vacuum environment, and the fluorine coating layer has a higher water drop contact angle to the process material than the surface of the main structure, the fluorine coating layer has a similar or higher hardness than the surface of the main structure, and the fluorine coating layer has a lower roughness than the surface of the main structure.
2. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The main structure is an outlet pipe of the process equipment or a pipe or component of a peripheral equipment of the process equipment.
3. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The fluorine coating layer is located on the surface of a portion of the main structure, and the portion is an inclined portion, a plane portion or a curved portion of the main structure.
4. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The fluorine coating layer has a higher acid corrosion resistance and a plasma etching resistance than the surface of the main structure.
5. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The surface of the main structure is roughened to form a rough surface with a rough structure, so as to increase the surface roughness.
6. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The surface of the main structure is treated by pickling or sandblasting to increase the surface roughness.
7. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The fluorine coating layer is composed of 0.01-20%wt of fluorocarbon compounds, 5-50%wt of alkoxysilanes, 0.01-20%wt of catalyst additives and 10-90%wt of solvents.
8. The anti-deposition article for use in a vacuum environment as claimed in claim 7, characterized in that: The fluorocarbon compound is selected from the group consisting of perfluoroalkanes, fluorochlorocarbons, semifluoroalkanes, fluoropolymers and hydrofluorochlorocarbons.
9. The anti-deposition article for use in a vacuum environment as claimed in claim 7, characterized in that: The fluorocarbon compound is a fluorine-containing monomer or polymer containing 1 to 20 carbon atoms.
10. The anti-deposition article for use in a vacuum environment as claimed in claim 7, characterized in that: The alkoxysilanes are selected from the group consisting of alkoxysilane oligomers, alkoxysilane compounds, alkoxysilane polymers, alkoxysiloxane oligomers, alkoxysiloxane compounds, alkoxysiloxane polymers, alkoxysilazane oligomers, alkoxysilazane compounds and alkoxysilazane polymers.
11. The anti-deposition article for use in a vacuum environment as claimed in claim 7, characterized in that: The catalytic additive is selected from the group consisting of metals, metal oxides, phosphates and carboxylates of platinum, titanium, tin, zinc, aluminum, silver, calcium, magnesium, potassium, sodium, nickel, chromium, molybdenum, vanadium, copper, iron, cobalt, germanium, hafnium, lanthanum, lead, ruthenium, tantalum, tungsten and zirconium.
12. The anti-deposition article for use in a vacuum environment as claimed in claim 7, characterized in that: The solvent is selected from the group consisting of alcohols, ketones, esters, fluoroalcohols, fluoroethers and ethers.
13. The anti-deposition article for use in a vacuum environment as claimed in claim 7, characterized in that: The alkoxysilane has a reactive functional group, and the reactive functional group undergoes a self-condensation reaction at room temperature for 1 to 7 days or at a temperature of 40 to 60 degrees Celsius for 1 to 24 hours.
14. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The process performed by the process equipment is an atomic layer deposition process, and the process material is titanium tetrachloride.
15. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The process performed by the process equipment is an organic metal chemical vapor deposition process, and the process material is a process gas or a process waste gas.
16. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The process performed by the process equipment is an aluminum pad process, and the process material is a process gas reactant or a process waste gas.
17. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The water drop contact angle of the fluorine coating layer ranges from 100 degrees to 120 degrees.
18. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The fluorine coating layer can withstand temperatures up to 600 degrees Celsius.
19. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The hardness of the fluorine coating layer ranges from 8H to 9H.
20. The anti-deposition article for use in a vacuum environment as claimed in claim 1, characterized in that: The adhesion between the fluorine coating layer and the surface of the main structure is in the range of 4B to 5B according to a hundred-grid test.