Preparation method of nano silicon carbide composite oxide film on surface of aluminum alloy

By forming a nano-silicon carbide composite oxide film on the surface of the aluminum alloy, the problem of insufficient hardness and wear resistance of the aluminum alloy in the existing technology is solved, and an aluminum alloy surface treatment with high hardness and wear resistance is achieved, which is suitable for high-demand applications. scene.

CN118773699APending Publication Date: 2024-10-15QUANZHOU INST OF INFORMATION ENG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410859406.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing aluminum alloy surface treatment methods cannot effectively improve the hardness and wear resistance, and are difficult to meet the high hardness and wear resistance requirements of engine cylinders and spinning machine spindles.

Method used

A method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy is adopted. By adding nano-silicon carbide particles in the hard anodizing process, using anionic surfactant and mechanical stirring and other technologies, the nano-silicon carbide particles enter the porous alumina. In the membrane pores, a composite oxide film with high hardness and wear resistance is formed.

Benefits of technology

It has achieved a significant improvement in surface hardness and wear resistance of aluminum alloy, making it suitable for high-demand applications such as engine cylinders and spinning machine spindles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773699A_ABST
    Figure CN118773699A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a nano silicon carbide composite oxide film on the surface of an aluminum alloy, which comprises the following steps: pretreating the surface of the aluminum alloy, dispersing nano silicon carbide particles in an aqueous solution of an anionic surfactant, and finally adding into an electrolyte of a hard anodic oxidation process to carry out hard oxidation on the aluminum alloy, thereby obtaining the nano silicon carbide composite oxide film on the surface of the aluminum alloy. And nano silicon carbide particles are co-deposited while the porous aluminum oxide film is generated, so that the nano silicon carbide composite oxide film is formed on the surface of the hard oxidized aluminum alloy. The preparation method is simple in process and good in repeatability, and the prepared nano silicon carbide composite oxide film is high in hardness and good in wear resistance and is expected to be applied to an engine cylinder and a spindle for a spinning machine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano materials, and in particular to a method for preparing a nano silicon carbide composite oxide film on the surface of an aluminum alloy. Background Art

[0002] Due to some disadvantages of aluminum and its aluminum alloys, such as low hardness, high friction coefficient and low corrosion resistance, their application is limited. The hard anodizing process of aluminum alloy is a simple, easy-to-operate and low-cost surface treatment method for aluminum alloy. The hardness obtained is significantly higher than that of untreated aluminum alloy or general anodized film, but it still cannot meet practical needs. For example, aluminum alloy has been used in engine cylinder materials, but due to its insufficient hardness and wear resistance, the life of the cylinder is not long. For another example, the high-speed rotating spindle in the spinning machine requires both good thermal conductivity and high hardness and good wear resistance. Aluminum alloy spindle is a potential excellent spindle material. Silicon carbide (SiC) is used in various types of production due to its good physical and chemical properties (such as high hardness, high wear resistance and good inert chemical behavior, etc.), which can make up for the shortcomings of aluminum alloy.

[0003] Ma Jun et al. (Corrosion and Protection, 2012, 33(9):784-79)1 reported that nano-silicon carbide was added to the electrolyte and composite anodized with 6061 aluminum alloy to obtain a composite oxide film, with a microhardness of 411 and a friction coefficient of about 0.19. The invention patent with publication number CN105586621A discloses a new aluminum alloy coating, in which the composite anodization includes a 15% sulfuric acid solution and n-SiC powder is added, the anodizing temperature is 22°C, and the oxidation time is 50min. However, according to the formula of the above literature or patent, it is difficult to successfully obtain a composite oxide film with SiC particles on the surface of the aluminum alloy. Therefore, it is of great significance to study a simple and reproducible method for preparing a nano-silicon carbide composite oxide film on the surface of the aluminum alloy. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy. The process is simple and has good repeatability. The prepared nano-silicon carbide composite oxide film has high hardness and good wear resistance, and is expected to be applied to engine cylinders and spindles for spinning machines.

[0005] In order to achieve the above object, the solution of the present invention is:

[0006] A method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy comprises the following steps:

[0007] Step 1: Aluminum alloy surface pretreatment:

[0008] First, the surface of the aluminum alloy is mechanically polished and degreased, then etched in nitric acid for 30 to 60 seconds, and then cleaned for later use;

[0009] Step 2: Cleaning of silicon carbide particles:

[0010] Then, the silicon carbide particles with an average particle size of 20 nm are added to hydrochloric acid for pickling, and then washed with deionized water for multiple times to remove impurities on the surface of the silicon carbide particles;

[0011] Step 3: Dispersion of silicon carbide particles:

[0012] Then, an anionic surfactant is added to deionized water and dissolved evenly to prepare a surfactant solution of 0.3-0.5 g / L. Then, the cleaned silicon carbide particles are added to the surfactant solution and ultrasonically dispersed for 30-90 minutes to obtain a suspension.

[0013] Step 4: Anodizing of aluminum alloy surface:

[0014] The dispersed suspension is then stirred again and added to the electrolyte. After continuous stirring for 30 to 60 minutes, hard anodization is performed using the surface pretreated aluminum alloy as the anode and the graphite plate as the cathode to obtain the nano-silicon carbide composite oxide film on the surface of the aluminum alloy.

[0015] In step 1, the aluminum alloy is 6061 aluminum alloy.

[0016] In step 1, the degreasing is performed by using alkaline solution.

[0017] In step 2, the mass ratio of the silicon carbide particles to the hydrochloric acid is 1-2:5, and the concentration of the hydrochloric acid is 50wt%.

[0018] In step 3, the anionic surfactant is one of sodium lauryl sulfate, sodium cetyl fatty acid and sodium octadecanoate.

[0019] In step 3, the amount of the silicon carbide particles added to the surfactant solution is 10 wt% to 15 wt% to ensure that the silicon carbide particles can reach adsorption saturation.

[0020] In step 4, after adding the suspension, the composition of the electrolyte includes 200 g / L sulfuric acid, 20 g / L oxalic acid, 20 g / L sulfosalicylic acid dihydrate, 3 g / L aluminum sulfate 18hydrate, and 2-6 g / L of silicon carbide particles treated with anionic surfactant.

[0021] In step 4, the process conditions of hard anodizing are: current density is 2-5A / dm 2, the electrolyte temperature is maintained at 5-10°C by circulating water cooling, and hard anodizing is carried out under the condition of mechanical stirring speed of 1000-2000 rpm for 30-60 min.

[0022] After adopting the above technical scheme, the present invention provides a method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy. By adding nano-silicon carbide particles to the electrolyte of the hard anodizing process, the aluminum alloy is hard-oxidized to generate a porous aluminum oxide film and nano-silicon carbide particles are co-deposited to form a composite oxide film to enhance the hardness and wear resistance of the oxide film layer.

[0023] The innovation of the method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy of the present invention is that in an electrolyte, nano-silicon carbide particles adsorb anionic surfactants and carry a partial negative charge, so that they migrate into the pores of a porous aluminum oxide film (pore size of about 30 nm) through mechanical and electrostatic effects during the subsequent hard anodizing process. Since the pore size of the porous aluminum oxide film of the aluminum alloy is larger than the average particle size of the silicon carbide particles (particle size of about 20 nm), the electrostatic effect prompts the silicon carbide particles with a partial negative charge to enter the pores of the porous aluminum oxide film, thereby forming a nano-silicon carbide composite oxide film.

[0024] The invention discloses a method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy. The process is simple, the properties of the electrolyte are stable, and the repeatability is good. The prepared nano-silicon carbide composite oxide film has high hardness and good wear resistance, and is expected to be applied to engine cylinders and spindles for spinning machines. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 XRD diagrams of ordinary aluminum alloy, the hard anodized aluminum alloy of Comparative Example 1, and the composite hard anodized aluminum alloy of Example 2;

[0026] Figure 2 These are scanning electron microscope images (SEM) of the hard anodized aluminum alloy of Comparative Example 1 and the composite hard anodized aluminum alloy of Example 2, wherein (a) is the hard anodized aluminum alloy at a magnification of 250 nm, (b) is the hard anodized aluminum alloy at a magnification of 500 nm, (c) is the composite hard anodized aluminum alloy at a magnification of 250 nm, and (d) is the composite hard anodized aluminum alloy at a magnification of 500 nm. DETAILED DESCRIPTION

[0027] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.

[0028] 1. Preparation of materials

[0029] Example 1

[0030] A method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy comprises the following steps:

[0031] Step 1: Aluminum alloy surface pretreatment:

[0032] The surface of the 6061 aluminum alloy was first mechanically polished, degreased with a 10wt% sodium hydroxide solution, then etched in 10wt% nitric acid for 30s, and then cleaned for later use;

[0033] Step 2: Cleaning of silicon carbide particles:

[0034] Then, according to a mass ratio of 1:5, silicon carbide particles with an average particle size of 20 nm were added to 50 wt % hydrochloric acid for pickling, and then washed with deionized water for multiple times to remove impurities on the surface of the silicon carbide particles;

[0035] Step 3: Dispersion of silicon carbide particles:

[0036] Then, sodium dodecyl sulfate was added into deionized water and dissolved evenly to prepare a surfactant solution with a concentration of 0.3 g / L, and then 10 wt % of the washed silicon carbide particles were added and ultrasonically dispersed for 30 min to obtain a suspension;

[0037] Step 4: Anodizing of aluminum alloy surface:

[0038] Then the dispersed suspension was stirred for 10 minutes and then added to the electrolyte. After continuous stirring for 30 minutes, the surface pretreated 6061 aluminum alloy was used as the anode and the graphite plate was used as the cathode for hard anodizing. The process conditions for hard anodizing were: current density of 3A / dm 2 , circulating water cooling is used to maintain the electrolyte temperature at 5°C, and hard anodizing is carried out under the condition of a mechanical stirring speed of 1000 rpm for 30 minutes, thereby obtaining a nano-silicon carbide composite oxide film on the surface of the aluminum alloy, that is, a composite hard oxide aluminum alloy with a nano-silicon carbide composite oxide film formed on the surface is obtained.

[0039] Among them, after adding the suspension, the composition of the electrolyte includes 200g / L sulfuric acid, 20g / L oxalic acid, 20g / L dihydrate sulfosalicylic acid, 3g / L aluminum sulfate 18hydrate, and 2g / L silicon carbide particles treated with anionic surfactant.

[0040] Example 2

[0041] A method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy comprises the following steps:

[0042] Step 1: Aluminum alloy surface pretreatment:

[0043] The surface of the 6061 aluminum alloy was first mechanically polished, degreased with a 10wt% sodium hydroxide solution, then etched in 10wt% nitric acid for 40s, and then cleaned for later use;

[0044] Step 2: Cleaning of silicon carbide particles:

[0045] Then, according to a mass ratio of 1:5, silicon carbide particles with an average particle size of 20 nm were added to 50 wt % hydrochloric acid for pickling, and then washed with deionized water for multiple times to remove impurities on the surface of the silicon carbide particles;

[0046] Step 3: Dispersion of silicon carbide particles:

[0047] Then, sodium dodecyl sulfate was added into deionized water and dissolved evenly to prepare a surfactant solution with a concentration of 0.4 g / L, and then 15 wt % of the washed silicon carbide particles were added and ultrasonically dispersed for 60 min to obtain a suspension;

[0048] Step 4: Anodizing of aluminum alloy surface:

[0049] Then the dispersed suspension was stirred for 10 minutes and then added to the electrolyte. After continuous stirring for 40 minutes, the surface pretreated 6061 aluminum alloy was used as the anode and the graphite plate was used as the cathode for hard anodizing. The process conditions for hard anodizing were: current density of 4A / dm 2 , circulating water cooling is used to maintain the electrolyte temperature at 10°C, and hard anodizing is carried out under the condition of a mechanical stirring speed of 1500 rpm for 40 minutes, thereby obtaining a nano-silicon carbide composite oxide film on the surface of the aluminum alloy, that is, a composite hard oxide aluminum alloy with a nano-silicon carbide composite oxide film formed on the surface is obtained.

[0050] Among them, after adding the suspension, the composition of the electrolyte includes 200g / L sulfuric acid, 20g / L oxalic acid, 20g / L dihydrate sulfosalicylic acid, 3g / L aluminum sulfate 18hydrate, and 4g / L silicon carbide particles treated with anionic surfactant.

[0051] Example 3

[0052] A method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy comprises the following steps:

[0053] Step 1: Aluminum alloy surface pretreatment:

[0054] The surface of the 6061 aluminum alloy was first mechanically polished, degreased with a 10wt% sodium hydroxide solution, then etched in 10wt% nitric acid for 60s, and then cleaned for later use;

[0055] Step 2: Cleaning of silicon carbide particles:

[0056] Then, according to a mass ratio of 2:5, silicon carbide particles with an average particle size of 20 nm were added to 50 wt % hydrochloric acid for pickling, and then washed with deionized water for multiple times to remove impurities on the surface of the silicon carbide particles;

[0057] Step 3: Dispersion of silicon carbide particles:

[0058] Then, hexadecanoic acid was added to deionized water and dissolved uniformly to prepare a surfactant solution with a concentration of 0.5 g / L, and then 15 wt% of the washed silicon carbide particles were added and ultrasonically dispersed for 90 minutes to obtain a suspension;

[0059] Step 4: Anodizing of aluminum alloy surface:

[0060] Then the dispersed suspension was stirred for 10 minutes and then added to the electrolyte. After continuous stirring for 60 minutes, the surface pretreated 6061 aluminum alloy was used as the anode and the graphite plate was used as the cathode for hard anodizing. The process conditions for hard anodizing were: current density of 5A / dm 2 , circulating water cooling is used to maintain the electrolyte temperature at 10°C, and hard anodizing is carried out under the condition of a mechanical stirring speed of 2000 rpm for 60 minutes, thereby obtaining a nano-silicon carbide composite oxide film on the surface of the aluminum alloy, that is, a composite hard oxide aluminum alloy with a nano-silicon carbide composite oxide film formed on the surface is obtained.

[0061] Among them, after adding the suspension, the composition of the electrolyte includes 200g / L sulfuric acid, 20g / L oxalic acid, 20g / L dihydrate sulfosalicylic acid, 3g / L aluminum sulfate 18hydrate, and 6g / L silicon carbide particles treated with anionic surfactant.

[0062] Comparative Example 1

[0063] A method for preparing an oxide film on the surface of an aluminum alloy comprises the following steps:

[0064] Step 1: Aluminum alloy surface pretreatment:

[0065] The surface of the 6061 aluminum alloy was first mechanically polished, degreased with a 10wt% sodium hydroxide solution, then etched in 10wt% nitric acid for 40s, and then cleaned for later use;

[0066] Step 2: Anodizing of aluminum alloy surface:

[0067] Then, the surface pretreated 6061 aluminum alloy was used as the anode and the graphite plate was used as the cathode for hard anodizing. The electrolyte composition included 200 g / L sulfuric acid, 20 g / L oxalic acid, 20 g / L sulfosalicylic acid dihydrate, and 3 g / L aluminum sulfate 18 hydrate. The process conditions for hard anodizing were: current density 4 A / dm 2 The electrolyte temperature was maintained at 10°C by circulating water cooling, and hard anodizing was carried out for 40 min under the condition of mechanical stirring speed of 1500 rpm, thereby obtaining an oxide film on the surface of the hard anodized aluminum alloy.

[0068] 2. Material Characterization

[0069] (1) XRD characterization

[0070] like Figure 1 As shown, the composite hard anodized aluminum alloy prepared in Example 2, the hard anodized aluminum alloy prepared in Comparative Example 1, and the pure aluminum alloy all have strong Al characteristic diffraction peaks at 2θ of about 38°, 44°, 65°, 78°, and 83°, wherein the hard anodized aluminum alloy and the composite hard anodized aluminum alloy both have a "steamed bun" peak in the range of 2θ of 20° to 30°, which indicates that the hard oxide film of the aluminum alloy is composed of amorphous Al2O3. The XRD spectrum of the composite hard anodized aluminum alloy shows a SiC characteristic diffraction peak, which proves that SiC nanoparticles exist on the surface of the composite hard anodized aluminum alloy.

[0071] (2) Scanning electron microscopy (SEM)

[0072] like Figure 2 As shown in (a) and (b), nanopores are evenly distributed on the surface of the anodized film of hard aluminum alloy, with a pore size of about 30nm, a relatively flat surface morphology, and good density. Figure 2 As shown in (c) and (d), SiC nanoparticles are attached to the surface and pores of the hard anodized aluminum alloy oxide film, and some SiC nanoparticles agglomerate. The above results show that SiC nanoparticles can effectively penetrate into the pores of the aluminum alloy oxide film, fill the pores, increase the surface density of the aluminum alloy, and play a role in improving the hardness.

[0073] 3. Performance Characterization

[0074] The microhardness of the composite hard anodized aluminum alloy prepared in each embodiment and the hard anodized aluminum alloy prepared in Comparative Example 1 was tested using a Vickers hardness tester, and the results are shown in Table 1. The results show that the hardness of the composite hard anodized aluminum alloy is relatively high.

[0075] Table 1 Hardness values ​​of composite hard anodized aluminum alloy and hard anodized aluminum alloy

[0076] Case Microhardness(Hv) Example 1 345 Example 2 387 Example 3 360 Comparative Example 1 294

[0077] The above embodiments and drawings do not limit the product form and style of the present invention. Any appropriate changes or modifications made by ordinary technicians in the relevant technical field should be deemed to be within the patent scope of the present invention.

Claims

1. A method for preparing nano-silicon carbide composite oxide film on aluminum alloy surface, Features: The following steps are involved: Step 1: Aluminum alloy surface pretreatment: First, the surface of the aluminum alloy is mechanically polished and degreased, then etched in nitric acid for 30 to 60 seconds, and then cleaned for later use; Step 2: Cleaning of silicon carbide particles: Then, the silicon carbide particles with an average particle size of 20 nm are added to hydrochloric acid for pickling, and then washed with deionized water for multiple times to remove impurities on the surface of the silicon carbide particles; Step 3: Dispersion of silicon carbide particles: Then, an anionic surfactant is added to deionized water and dissolved evenly to prepare a surfactant solution of 0.3-0.5 g / L. Then, the cleaned silicon carbide particles are added to the surfactant solution and ultrasonically dispersed for 30-90 minutes to obtain a suspension. Step 4: Anodizing of aluminum alloy surface: The dispersed suspension is then stirred again and added to the electrolyte. After continuous stirring for 30 to 60 minutes, hard anodization is performed using the surface pretreated aluminum alloy as the anode and the graphite plate as the cathode to obtain the nano-silicon carbide composite oxide film on the surface of the aluminum alloy.

2. The method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy according to claim 1, Features: In step 1, the aluminum alloy is 6061 aluminum alloy.

3. The method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy according to claim 1, Features: In step 1, the degreasing is performed by using alkaline solution.

4. The method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy according to claim 1, Features: In step 2, the mass ratio of the silicon carbide particles to the hydrochloric acid is 1-2:5, and the concentration of the hydrochloric acid is 50wt%.

5. The method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy according to claim 1, Features: In step 3, the anionic surfactant is one of sodium lauryl sulfate, sodium cetyl fatty acid and sodium octadecanoate.

6. The method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy according to claim 1, Features: In step 3, the amount of silicon carbide particles added to the surfactant solution is 10 wt% to 15 wt%.

7. The method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy according to claim 1, Features: In step 4, after adding the suspension, the composition of the electrolyte includes 200 g / L sulfuric acid, 20 g / L oxalic acid, 20 g / L sulfosalicylic acid dihydrate, 3 g / L aluminum sulfate 18hydrate, and 2-6 g / L of silicon carbide particles treated with anionic surfactant.

8. The method for preparing a nano-silicon carbide composite oxide film on the surface of an aluminum alloy according to claim 1, Features: In step 4, the process conditions of hard anodizing are: current density is 2-5A / dm 2 , the electrolyte temperature is maintained at 5-10°C by circulating water cooling, and hard anodizing is carried out under the condition of mechanical stirring speed of 1000-2000 rpm for 30-60 min.