Elastic mixed fiber false twist processed yarn, preparation method thereof and fabric
By using polyamide filament and polyester fully drawn yarn in the mixed fiber processing yarn, adjusting the crimp structure and heat treatment, the problems of color mixing effect and insufficient resilience in the existing technology are solved, and high resilience and anti-permeability are achieved of functional fabrics.
Patent Information
- Application Number
- CN202310350272.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-15
AI Technical Summary
The existing mixed fiber processed yarn has a weak color mixing effect after dyeing and lacks excellent fabric resilience, making it unable to meet higher quality requirements.
Using mixed fiber false twisted processed yarn composed of polyamide filament and polyester fully drawn yarn, by adjusting the crimp structure and content of the core yarn and sheath yarn, combined with heat treatment and network device technology, it forms a shape with excellent stretch and elongation. Mixed fiber yarn with recovery properties.
It is a functional fabric that achieves high resilience, anti-permeability and meta-dying effect. It has good color mixing effect and hand feel, and is suitable for high-quality T-shirts and casual clothing.
Smart Images

Figure CN118773787A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a mixed-fiber false-twist processed yarn, in particular to a mixed-fiber false-twist processed yarn formed by polyamide filaments and polyester fully drawn yarns and having the effects of resilience, anti-permeability, and abnormal dyeing. Background Art
[0002] The fabric is made of a blended yarn of polyester fiber with stretchable recovery and nylon fiber with high titanium dioxide content. It has the vertical and cool feeling of nylon, as well as the high elasticity, dimensional stability and ironing-free properties of polyester. It is also anti-transparent and anti-ultraviolet, and has a significant mixed-color flash effect after dyeing. It is an ideal new fabric, especially suitable for T-shirts and casual wear, and has broad market prospects.
[0003] Chinese patent CN107532345A discloses a mixed fiber processing filament composed of polyamide filament and polyester filament, wherein the difference in length between the polyamide filament and the polyester filament in the mixed fiber processing filament is 5-30%. Although the mixed fiber processing filament has a different color effect after dyeing, the color mixing effect is weak due to the small difference in length between the polyamide filament and the polyester filament, and there is no excellent fabric rebound effect, which cannot meet people's pursuit of higher quality requirements.
[0004] Therefore, it is necessary to design a composite mixed fiber yarn that has a strong color mixing effect, a good cool feeling and a good vertical feeling, and can also meet the requirements of good resilience and high anti-transmission. Summary of the invention
[0005] The object of the present invention is to provide a mixed fiber false twisted textured yarn with stretchability and elongation and a preparation method thereof. The mixed fiber false twisted textured yarn can be applied to functional fabrics requiring vertical feeling, cool feeling, anti-dyeing and high resilience.
[0006] The technical solution of the present invention is: The elastic mixed fiber false twist processed yarn is composed of a core yarn and a sheath yarn, and both the core yarn and the sheath yarn have a curling structure. The core yarn is a polyamide filament, and the sheath yarn is a polyester fully drawn yarn; the curling radius of the sheath yarn is 0.3-1.5 mm, and the ratio of the curling radius of the core yarn to the curling radius of the sheath yarn is 3-16.
[0007] The polyester fully drawn yarn is preferably a composite component of normal pressure cationic dyeable polyester and polybutylene terephthalate, and the stretch elongation is preferably 15-25%.
[0008] The titanium dioxide content in the polyamide filaments is preferably above 2.0 wt %.
[0009] The elastic mixed fiber false twisted yarn preferably has a stretch elongation of 15 to 35%, more preferably 20 to 30%, and a stretch recovery rate of 80 to 90%.
[0010] The present invention also discloses a method for preparing the elastic mixed fiber false twist processed yarn, wherein the polyamide filament is drawn through the first roller, heated through the first heat box, introduced into the false twister, enters the second roller, and then enters the networker together with the polyester fully drawn yarn that has passed through the zero roller for doubling, and then sequentially passes through the second heat box, the third roller, and finally is wound at the winding roller to obtain the mixed fiber yarn. The temperature of the first heat box is 150-220°C.
[0011] The network device is preferably a network device with a 2-hole spiral guide, and the pressure at the network device is preferably 1.5-5.0 kg / cm 2 .
[0012] The elastic mixed fiber false twist processed yarn of the present invention can be used to make fabrics, and the fabrics made therefrom have the characteristics of vertical feeling, strong cool feeling, anti-dyeing and high resilience. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a schematic engineering diagram of the method for preparing the elastic mixed fiber false twist processed yarn of the present invention.
[0014] Figure 2 This is a schematic diagram of the curling radius of elastic blended false-twist processed yarn. DETAILED DESCRIPTION
[0015] The elastic blended false-twist processed yarn of the present invention is composed of a core yarn and a sheath yarn. The core yarn is a polyamide filament, which is made of any of ordinary nylon polymers such as nylon 6, nylon 56, and nylon 66. The present invention does not specifically limit the content of polyamide filaments in the elastic blended false-twist processed yarn, but if the content of the polyamide filaments is too low, the coolness and drape of the resulting fabric decrease; when the content of the polyamide filaments is too high, the elasticity of the resulting fabric is insufficient. The content of polyamide filaments in the elastic blended false-twist processed yarn of the present invention is preferably 10 to 50 wt%.
[0016] The sheath yarn is a polyester fully drawn yarn. Polyamide is an acid dyeable polymer, and polyester is an acid non-dyeable polymer. The dyeing mechanisms of the two are different, so after dyeing with one dye, a meta-dyeing effect will be produced.
[0017] The invention limits the curling radius of the sheath yarn in the elastic mixed fiber false twist processed yarn to 0.3-1.5 mm, and the ratio of the curling radius of the core yarn to the curling radius of the sheath yarn to be within the range of 3-16, so that the obtained elastic mixed fiber false twist processed yarn has excellent telescopic elongation and elongation recovery characteristics after heat treatment, and the obtained fabric has good elastic effect, can achieve excellent color mixing effect and excellent hand feeling. The smaller the ratio of the curling radius of the core yarn to the curling radius of the sheath yarn, the closer the curling form of the core yarn is to the curling form of the sheath yarn, and the overall processed yarn cannot achieve the required elongation and recovery characteristics, and the elasticity of the fabric is not good. Therefore, if the ratio of the curling radius of the core wire to the curling radius of the sheath wire is less than 3, or the curling radius of the sheath wire is greater than 1.5 mm, the elastic elongation of the elastic blended false twisted yarn is low, and the elastic effect of the fabric becomes poor; if the ratio of the curling radius of the core wire to the curling radius of the sheath wire is greater than 16, or the curling radius of the sheath wire is less than 0.3 mm, although the elastic effect of the fabric is good, the sheath wire forms self-curling due to the small curling radius, and it is easy to form small braids on the fabric, affecting the quality. In order to achieve the best elastic effect of the final fabric, the present invention preferably has a curling radius of 0.5 to 1.0 mm for the sheath wire, and a ratio of the curling radius of the core wire to the curling radius of the sheath wire of 5 to 12.
[0018] The sheath yarn is preferably an elastic parallel composite fiber, and the specific elasticity can be characterized by the stretching elongation. The higher the stretching elongation of the polyester fully drawn yarn, the smaller the curling radius of the sheath yarn, the better the elasticity of the fabric, but the poor productivity; the lower the stretching elongation of the polyester fully drawn yarn, the larger the curling radius of the sheath yarn, the smaller the curling radius ratio of the core yarn to the sheath yarn, and the worse the elasticity of the fabric. In order to make the sheath yarn form a curl of appropriate size, the stretching elongation of the polyester fully drawn yarn is preferably 15-25%.
[0019] The specific parallel composite polymers can be PET / PBT, high viscosity PET / low viscosity PET, PET / PTT, normal pressure cation dyeable PET / PBT, etc. Since normal pressure cation dyeable polyester can provide a more natural mixed color style, normal pressure cation dyeable PET / PBT parallel composite fibers are preferred.
[0020] In the present invention, the polyamide filaments preferably contain 2 wt % of titanium dioxide, so that the resulting fabric has good anti-transmission and anti-ultraviolet effects.
[0021] The core yarn and the sheath yarn of the elastic mixed fiber false twist processed yarn of the present invention both have a curled shape, and the overall processed yarn has good expansion and contraction elongation. The expansion and contraction elongation after heat treatment can reach 15-35%, preferably 20-30%, and the elongation recovery rate can reach 80-90%.
[0022] The elastic mixed fiber false twist processed yarn of the present invention can be obtained by the following method: firstly, the polyamide filament is drawn by the first roller, heated by the first heat box, introduced into the false twister, enters the second roller, and then enters the network device together with the polyester full-drawn yarn passing through the zero roller for winding, and then passes through the second heat box, the third roller, and finally winds up at the winding roller to obtain the mixed fiber yarn. By inserting the sheath yarn later, the processed yarn can form a uniform mixed color dyeing effect.
[0023] At the same time, the polyamide filaments are more elastic after false twist heat treatment, and the core filaments can obtain a certain curling radius by adjusting the temperature of the first hot box during the false twist process. When the temperature of the first hot box is lower than 150°C, the curling radius of the core filament is too large, and the elasticity is lower, which affects the elasticity of the processed yarn and subsequent fabrics; when the temperature of the first hot box is higher than 220°C, although the curling radius of the core filament is small, the elasticity of the mixed fiber false twist processed yarn is high, and the fabric has good elasticity, the polyamide filaments are also prone to melting, resulting in a hard feel of the final fabric.
[0024] The present invention does not limit the type of network device used for the combined yarn. In order to improve the uniformity of dyeing, the present invention preferably uses a 2-hole gyratory network device, and the pressure of the network device is preferably 1.5-5.0 kg / cm 2 .
[0025] The present invention uses polyamide filaments as core yarns and elastic polyester fully drawn yarns as sheath yarns, and the dyeing mechanisms of the two are different, so that the fabric finally obtained can obtain advanced color mixing effect and stretching and elongation compacting effect. In the preferred technical solution, the fabric also has the characteristics of anti-transmission and anti-ultraviolet properties.
[0026] The test method involved in the present invention is as follows: (1) Elongation and recovery of processed yarn Telescopic elongation (%) = ((L1-L0) / L0)*100%, Elongation recovery rate (%) = ((L1-L2) / (L1-L0))*100%, L0: The length of the fiber measured after it is treated with 90-degree hot water for 2 minutes under a load of 2 mg / d and then hung to dry for 12 hours is L0; L1: After L0 measurement, remove the initial load during L0 measurement, and hang a fixed load of 100 mg / d after 2 minutes. The length measured after 30 seconds is L1; L2: After L1 is measured, remove the fixed load used in the L1 measurement, and then apply an initial load of 2 mg / d after 2 minutes. The length measured after 30 seconds is L2.
[0027] (2) Calculation of the curling radius of mixed yarn a. Take 5 mixed fiber false twisted yarns of the same length on the measuring machine.
[0028] b. Extract 5 single filament bundles of core polyamide filament and sheath polyester fully drawn filament from the mixed fiber false twisted yarn respectively.
[0029] c. Apply a load tension of 1 / 10 dtex × 0.18 mN / dtex to the obtained yarn bundle, and after 5 minutes, stick the yarn bundle on a special black paper in its natural state.
[0030] d. Use a microscope to measure the curling diameter R of the core wire and sheath wire respectively, unit: mm (microscope model: Keyence VHX-2000) e. Calculate the curling radius r of the core wire and sheath wire respectively, and find the average value of each radius (r=R / 2) f. The final calculated curling radius ratio = core wire curling radius / sheath wire curling radius.
[0031] (3) Spinnability Spinning property refers to the process of mixing fibers. The fewer broken wires appear within 12 hours, the lower the broken wire rate, indicating better spinning property; the higher the broken wire rate, the worse the spinning property. No broken wire within 12 hours is judged as excellent and marked with ○; the broken wire rate within 12 hours is 5-10%, which is judged as good and marked with △; the broken wire rate within 12 hours is greater than 10%, which is judged as poor and marked with ×.
[0032] Broken wire rate = (number of broken wires / number of hanging wires) * 100% (calculated after 12 hours).
[0033] (4) Metachromatic effect The mixed fiber processed filaments are woven into fabrics, and the surface of the fabrics is observed after dyeing with two dyes. Uneven dyeing and obvious light and dark dyeing mixed color effects indicate that there is a different color effect, and uniform dyeing and full dyeing indicate that there is no different color effect. Ten people with experience in this field judge the appearance of the fabric. If 6 to 9 people think that the natural mixed color feeling is uniform, it is judged as ○, 6 to 9 people think that the stripes are obvious and the natural mixed color feeling is average, it is judged as △, and 6 to 9 people think that the pockmarks are obvious and the natural mixed color feeling is poor, it is judged as ×.
[0034] (5) Shading effect Use a color tone meter to test the L value of a white board and a black board: L (white), L (black). Take a fabric sample (10×10cm) and test the L value against a white board and a black board: L (white + fabric), L (black + fabric). Light transmittance: (1-(L(white+cloth)-L(black+cloth)) / (L(white)-L(black))×100%.
[0035] A transmittance lower than 70% indicates poor anti-transmission effect, which is judged as ×; a transmittance between 70% and 80% indicates good effect, which is judged as △; a transmittance greater than 80% indicates excellent effect, which is judged as ○.
[0036] (6) Fabric elasticity Measured according to JISL 1096:2010A standard.
[0037] The elastic elongation and elastic recovery of the fabric in the elastic direction were measured, and the average value was calculated based on 5 measurements of each data. If the elastic elongation is less than 5% or the elastic recovery is less than 80%, it is judged as ×; if the elastic elongation is 5-15% and the elastic recovery is 80-95%, it is judged as △; if the elastic elongation is 15%-25% and the elastic recovery is 80%-95%, it is judged as ○; if the elastic elongation is greater than 25% and the elastic recovery is 80%-95%, it is judged as ◎.
[0038] The present invention is described in more detail below with reference to the embodiments, but the embodiments are not intended to limit the present invention.
[0039] Embodiment 01
[0040] The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 160°C, and then sequentially introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 20% is passed from the same spindle position through the zero roller into the second roller, and after being combined with the polyamide filament, it enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0041] Embodiment 02
[0042] The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 150°C, and then successively introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 20% is passed from the same spindle position through the zero roller into the second roller, and after being combined with the polyamide filament, it enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0043] Embodiment 03
[0044] The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 220°C, and then successively introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 20% is passed from the same spindle position through the zero roller into the second roller, and after being combined with the polyamide filament, it enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0045] Embodiment 04
[0046] The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 160°C, and then sequentially introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 15% is passed from the same spindle position through the zero roller into the second roller, and after being combined with the polyamide filament, it enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0047] Embodiment 05
[0048] The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 160°C, and then successively introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 25% is passed from the same spindle position through the zero roller into the second roller, and after being combined with the polyamide filament, it enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0049] Embodiment 06
[0050] The polyamide nylon 6 filament with a titanium dioxide content of 0.3% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 160°C, and then sequentially introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 20% enters the second roller through the zero roller from the same spindle position, and after being combined with the polyamide filament, enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0051] Embodiment 07
[0052] The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 160°C, and then successively introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 13% is passed from the same spindle position through the zero roller into the second roller, and after being combined with the polyamide filament, it enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0053] Embodiment 08
[0054] The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 160°C, and then successively introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 27% is passed from the same spindle position through the zero roller into the second roller, and after being combined with the polyamide filament, it enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0055] Embodiment 09
[0056] The polyamide nylon 66 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 160°C, and then successively introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 20% is passed from the same spindle position through the zero roller into the second roller, and after being combined with the polyamide filament, it enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0057] Example 10
[0058] The polyester filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 160°C, and then successively introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 20% enters the second roller through the zero roller from the same spindle position, and after being combined with the polyester filament, enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0059] Embodiment 11
[0060] The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 160°C, and then sequentially introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the high-viscosity PET / low-viscosity PET composite parallel full-drawn filament with a stretch elongation of 20% enters the second roller through the zero roller from the same spindle position, and after being combined with the polyamide filament, enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0061] Example 12
[0062] The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 160°C, and then sequentially introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the PET / PTT composite parallel full-drawn filament with a stretching elongation of 20% enters the second roller from the same spindle position through the zero roller, and after being combined with the polyamide filament, enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0063] Comparative Example 01 The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 140°C, and then sequentially introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 20% is passed from the same spindle position through the zero roller into the second roller, and after being combined with the polyamide filament, it enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0064] Since the temperature of the first heat box is too low, the final processed yarn has low elongation and the fabric has poor elasticity.
[0065] Comparative Example 02 The polyamide nylon 6 filament with a titanium dioxide content of 2.2% is fed into the first roller, passed through the first hot box, wherein the temperature of the first hot box is set to 230°C, and then successively introduced into the false twister, and then entered the second roller for stretching and false twisting at a processing speed of 500m / min, and then the modified normal pressure cationic dyeable PET / PBT composite parallel full-drawn filament with a stretch elongation of 20% enters the second roller through the zero roller from the same spindle position, and after being combined with the polyamide filament, enters the network device with a 2-hole convolute guide, and enters the third roller to obtain the mixed fiber false twist processed yarn. Other specific properties are shown in Table 1.
[0066] Since the temperature of the heating box 1 is too high, the polyamide core yarn melts and the spinnability is poor.
[0067]
Claims
1. Elastic mixed fiber false twist processed yarn, composed of core yarn and sheath yarn, both of which have a curled structure, characterized in that: The core yarn is a polyamide filament, and the sheath yarn is a polyester fully drawn yarn; the curling radius of the sheath yarn is 0.3-1.5 mm, and the ratio of the curling radius of the core yarn to the curling radius of the sheath yarn is 3-16.
2. The elastic blended false twisted yarn according to claim 1, characterized in that: The polyester fully drawn yarn is a composite component of normal pressure cationic dyeable polyester and polybutylene terephthalate, and has a stretching elongation of 15-25%.
3. The elastic blended false twisted yarn according to claim 1, characterized in that: The titanium dioxide content in the polyamide filament is above 2.0wt%.
4. The elastic blended false twisted yarn according to claim 1, characterized in that: The elastic mixed fiber false twist processed yarn has a stretching elongation of 15-35% and an elongation recovery rate of 80-90%.
5. The elastic mixed fiber false twisted yarn according to claim 4, characterized in that: The elastic mixed fiber false twist processed yarn has a stretching elongation of 20 to 30%.
6. The method for preparing the mixed elastic mixed fiber false twist processed yarn according to claim 1, wherein the polyamide filament is drawn by the first roller, heated by the first heat box, introduced into the false twister, enters the second roller, and then enters the networker together with the polyester fully drawn yarn that has passed the zero roller for doubling, and then passes through the second heat box, the third roller in sequence, and finally is wound at the winding roller to obtain the mixed fiber yarn, characterized in that: The temperature of the first heat box is 150-220°C.
7. A fabric mainly made from the mixed false-twisted yarn according to claim 1.
Citation Information
Patent Citations
Blended yarn processing filament and fabric prepared by same
CN106283305A
Preparation method of two-component composite wool-like elastic fiber
CN111379048A
Multicolor dyeable composite false twisted yarn and method for producing the same
JP2008025043A
Composite drawn false twisted yarn
JP2012211423A
Bulky yarn
US20180216261A1