Method for preparing nanocellulose by treating bamboo shoot shells with deep-eutectic solvent

The nanocellulose in the bamboo shoot shells is extracted through the synergistic cooperation of the ternary deep eutectic solvent and the cosolvent, which solves the problems of high equipment, high cost and environmental pollution in the existing technology, and realizes the preparation of nanocellulose with high efficiency and low energy consumption. Moreover, the size of nanocellulose can reach 58.78nm, and the yield and proportion are high.

CN118773940AActive Publication Date: 2024-10-15INST AGRO PROD PROCESSING ANHUI ACADEMY AGRI SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410987558.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-15
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing methods for extracting nanocellulose from bamboo shoot shells have problems such as high equipment requirements, high costs, high energy consumption, and serious environmental pollution. In particular, high-pressure homogenization methods and chemical methods have a greater negative impact on the environment, and biological methods and enzymatic hydrolysis methods operate Complex and costly.

Method used

The ternary deep eutectic solvent and co-solvent are used to extract nanocellulose, and the removal rate of lignin and hemicellulose is improved through the coordination of metal salts, and smaller-sized nanocellulose crystals are obtained under low temperature conditions. Utilizing benzyl tripropyl ammonium hydroxide and 1'3-bishydroxymethylurea to improve the solubility and recovery of cellulose molecules.

Benefits of technology

Achieving high yield (88.36%) and high cellulose proportion (90.19%), obtaining nanocellulose at a lower temperature, simplifying the process, reducing energy consumption and environmental pollution, and improving reaction speed and solvent efficiency Recycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773940A_ABST
    Figure CN118773940A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing nanocellulose by treating bamboo shoot shells with a deep-eutectic solvent, which comprises the following steps: S1, preparation of the deep-eutectic solvent: uniformly mixing a first component, a second component and a third component, stirring and heating to obtain a ternary deep-eutectic solvent; s2, preparation of a cosolvent: uniformly mixing benzyltripropylammonium hydroxide, 1 '3-bis (hydroxymethyl) urea and water, stirring and heating to obtain the cosolvent; s3, preparation of nanocellulose: mixing the pretreated bamboo shoot shell, the ternary eutectic solvent and the cosolvent, stirring and heating, after the reaction is finished, washing, performing suction filtration and drying to obtain a cellulose crude product, preparing the cellulose crude product into turbid liquid, and performing ultrasonic treatment, high-pressure homogenization and freeze-drying to obtain the nanocellulose. The nanocellulose obtained after treatment by the method disclosed by the invention is high in yield (88.36%) and high in cellulose proportion (90.19%), and the size of the nanocellulose can reach 58.78 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cellulose, and in particular to a method for preparing nanocellulose by treating bamboo shoot shells with a low eutectic solvent. Background Art

[0002] Nanocellulose, with its unique lignin composition and nanoscale characteristics, has shown broad application prospects in many fields such as automotive lightweighting, papermaking, food packaging, textile fabrics, biomedicine, and lignin modification. It can not only effectively reduce the weight of automotive components, improve paper performance, and create high-strength and high-transparency food packaging, but also give textile fabrics a variety of functional properties, and serve as a carrier for biodegradable materials and drug delivery systems in the biomedical field. In addition, nanocellulose has shown great potential in the field of flexible electronics in terms of electrochemical performance and mechanical stability.

[0003] Bamboo shoots are an important green food and economic crop. my country is rich in bamboo shoot resources, and the southern mountainous area of ​​Anhui Province is one of the main production areas of bamboo shoots. During the bamboo shoot processing season every year, a large amount of processing by-products pile up and are not effectively utilized, resulting in a waste of resources. Bamboo shoot shells, as a by-product of bamboo shoot processing, account for 30%-40% of the whole bamboo shoots and are mainly composed of cellulose, hemicellulose and lignin. Using this as a raw material for extracting nanocellulose is a utilization of agricultural waste, which has a positive role in promoting green environmental protection.

[0004] At present, there are many methods for extracting nanocellulose from bamboo shoots, including physical, chemical, biological and enzymatic methods. The most commonly used physical method is high-pressure homogenization extraction, but it has high equipment requirements and costs, and consumes a lot of energy; the chemical method mainly uses acid, alkali and TEMPO to extract, but due to the corrosiveness of the solvent, it cannot be recovered in the later stage and has a great pollution to the environment; the biological method degrades the cellulose in bamboo shoots through microbial fermentation, but the operating conditions are complicated; although the enzymatic method is simple to operate and environmentally friendly, it has high requirements for the reaction solvent and ambient temperature, and the reaction time is long and the cost is high. Summary of the invention

[0005] In order to solve the problems mentioned in the above background technology, the present invention provides a method for preparing nanocellulose by treating bamboo shoot shells with a low eutectic solvent.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions: A method for preparing nanocellulose by treating bamboo shoot shells with a deep eutectic solvent comprises the following steps: S1. Configuration of deep eutectic solvent: After the first component, the second component and the third component are uniformly mixed, they are stirred and heated to obtain a ternary deep eutectic solvent; S2. Configuration of co-solvent: Benzyltripropylammonium hydroxide, 1'3-bis(hydroxymethyl)urea and water are uniformly mixed, stirred and heated to obtain a cosolvent; S3. Preparation of Nanocellulose: The pretreated bamboo shoot shells, ternary low eutectic solvent and co-solvent are mixed, stirred and heated, and after the reaction is completed, washed with water, filtered and dried to obtain crude cellulose. The crude cellulose is configured into a suspension, ultrasonicated, high-pressure homogenized and freeze-dried to obtain nanocellulose.

[0007] Preferably, the first component is choline chloride, the second component is glycerol or oxalic acid, and the third component is any one of aluminum chloride hexahydrate, ferric chloride hexahydrate, and zinc chloride hexahydrate.

[0008] Preferably, the molar ratio of the first component, the second component and the third component is 1:1:(0.1-0.3).

[0009] Preferably, the mass ratio of the benzyltripropylammonium hydroxide, 1'3-bis(hydroxymethyl)urea and water is 1:1:(10-20).

[0010] Preferably, the method of pre-treating bamboo shoot shells is: The bamboo shoot shells were cleaned, dried, cut, and crushed through an 80-mesh sieve to obtain the original sample, referred to as OS; OS was mixed with deionized water in a mass ratio of 1:10, stirred continuously at 90 °C for 2 h, with a rotation speed of 800 rpm, filtered using a 200-mesh sieve, and the solid insoluble matter was placed in an oven and dried at 60 °C for 5 h; The preliminarily treated dry powder was mixed with a 1% NaOH solution at a mass ratio of 1:10, and stirred continuously at 90°C for 2 h at a rotation speed of 800 rpm. After the stirring, it was filtered through a 200-mesh sieve, and the filtered solid was washed with deionized water until the pH of the filtrate was close to neutral. The solid was dried at 60°C for 5 h, and then crushed through an 80-mesh sieve to obtain the pretreated bamboo shoot shell, referred to as PS.

[0011] Preferably, the mass ratio of the pretreated bamboo shoot shell, the ternary low eutectic solvent and the co-solvent is (1-10):100:(10-20).

[0012] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses a ternary deep eutectic solvent and a co-solvent to extract nanocellulose. Compared with the existing binary deep eutectic solvent, the present invention introduces a third component metal salt, and the metal coordination effect formed improves the removal rate of lignin and hemicellulose, and improves the yield of nanocellulose in bamboo shoot shells. In a short time, nanocellulose crystals of smaller size can be obtained at a lower temperature. Compared with the binary deep eutectic solvent, the eutectic point of the ternary deep eutectic solvent is lower, which can improve the reaction speed and yield. The ternary deep eutectic solvent can reach a melting point under low temperature conditions due to more components, has better conductivity and solubility, and is more convenient for the recycling of later solvents.

[0013] 2. The present invention simultaneously introduces benzyltripropylammonium hydroxide and 1'3-bis(hydroxymethyl)urea. The hydroxide on the benzyltripropylammonium hydroxide can generate hydrogen bonds with the hydroxyl groups on the cellulose, thereby changing the original intermolecular and intramolecular hydrogen bonds of the cellulose; the amino groups and hydroxyl groups on the 1'3-bis(hydroxymethyl)urea molecules can form hydrogen bonds with the benzyltripropylammonium hydroxide, and then form composite hydrated ions with water molecules, which are coated on the surface of the cellulose molecular chains, thereby preventing the aggregation of the cellulose molecular chains and promoting the dispersion of the cellulose.

[0014] 3. The nanocellulose obtained after being treated by the method of the present invention has a high yield (88.36%), a high cellulose content (90.19%), and a size of up to 58.78 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is a transmission electron microscope image of Example 1 (CGF); Figure 2 is a transmission electron microscope image of Example 2 (COF); Figure 3 is a transmission electron microscope image of Example 3 (COA); Figure 4 This is a transmission electron microscope image of Example 4 (COZ). DETAILED DESCRIPTION

[0016] Unless otherwise specified, the raw materials and reagents used in the present invention are commercially available or can be prepared by known methods.

[0017] The method of pre-treating bamboo shoot shells is: The bamboo shoot shells were cleaned, dried, cut, and crushed through an 80-mesh sieve to obtain the original sample, referred to as OS; OS was mixed with deionized water in a mass ratio of 1:10, stirred continuously at 90 °C for 2 h, with a rotation speed of 800 rpm, filtered using a 200-mesh sieve, and the solid insoluble matter was placed in an oven and dried at 60 °C for 5 h; The preliminarily treated dry powder was mixed with a 1% NaOH solution at a mass ratio of 1:10, and stirred continuously at 90°C for 2 h at a rotation speed of 800 rpm. After the stirring, it was filtered through a 200-mesh sieve, and the filtered solid was washed with deionized water until the pH of the filtrate was close to neutral. The solid was dried at 60°C for 5 h, and then crushed through an 80-mesh sieve to obtain the pretreated bamboo shoot shell, referred to as PS. Example 1

[0018] A method for preparing nanocellulose by treating bamboo shoot shells with a deep eutectic solvent, characterized in that it comprises the following steps: S1. Configuration of deep eutectic solvent: Choline chloride, glycerol and ferric chloride hexahydrate were mixed uniformly in a molar ratio of 1:1:0.2, and stirred at 80° C. until a uniform transparent solution was obtained to obtain a ternary deep eutectic solvent; S2. Configuration of co-solvent: Benzyltripropylammonium hydroxide, 1'3-bis(hydroxymethyl)urea and water were mixed uniformly in a mass ratio of 1:1:15, and stirred at 60° C. until a uniform transparent solution was obtained to obtain a cosolvent; S3. Preparation of Nanocellulose: The pretreated bamboo shoot shells, ternary low eutectic solvent and co-solvent were mixed in a mass ratio of 5:100:15, stirred at 90°C for 2h, washed with water, filtered, and dried at 60°C to obtain crude cellulose. The crude cellulose was prepared into a 0.5wt% suspension, treated with ultrasound at 700w for 30min, and treated with high-pressure homogenization at 400Mpa for 5min to obtain a nanocellulose suspension, which was freeze-dried with a freeze dryer to obtain nanocellulose, referred to as CGF. Example 2

[0019] The difference between this embodiment and the embodiment is: Choline chloride, oxalic acid and ferric chloride hexahydrate were mixed uniformly in a molar ratio of 1:1:0.2, and stirred at 80° C. until a uniform transparent solution was obtained to obtain a ternary deep eutectic solvent; The rest is exactly the same as in Example 1; The resulting nanocellulose is referred to as COF. Example 3

[0020] The difference between this embodiment and the embodiment is: Choline chloride, oxalic acid and aluminum chloride hexahydrate were mixed uniformly in a molar ratio of 1:1:0.2, and stirred at 80° C. until a uniform transparent solution was obtained to obtain a ternary deep eutectic solvent; The rest is exactly the same as in Example 1; The obtained nanocellulose is referred to as COA. Example 4

[0021] The difference between this embodiment and the embodiment is: Choline chloride, oxalic acid and zinc chloride hexahydrate were mixed uniformly in a molar ratio of 1:1:0.2, and stirred at 80° C. until a uniform transparent solution was obtained to obtain a ternary deep eutectic solvent; The rest is exactly the same as in Example 1; The resulting nanocellulose is referred to as COZ.

[0022] Results and Testing Nanocellulose yield and chemical composition analysis Use the weighing method to weigh the mass of the pre-treated bamboo shoots (m 0 ) and the mass of bamboo shoot shell after treatment with deep eutectic solvent (m 1 ), through the formula C=(m 1 / m 0 )*100%, calculate the yield; The chemical composition of bamboo shoot shells was analyzed by UV spectrophotometer according to the U.S. Department of Energy Renewable Energy Laboratory method (NREL, 2008) and kit; The morphology of the bamboo shoot shell was observed by transmission electron microscopy and the particle size was calculated, as shown in Table 1.

[0023] Table 1

[0024] Application of preparing nanocellulose by treating bamboo shoot shell with deep eutectic solvent A preparation method of a modified PVA composite film comprises the following steps: Preparation of modified nanocellulose: The nanocellulose (CGF) prepared in Example 1 and water were ultrasonically homogenized into a suspension with a mass fraction of 5%, 0.1 mol / L HCl was prepared to adjust the pH of the suspension to 4, and the suspension was stirred in a water bath at 100°C for 10 min, and then a citric acid solution with a mass fraction of 2% was added to control the pH to 3-4, and the suspension was stirred in a water bath at 100°C for 2 h. After cooling to room temperature, the suspension was dialyzed to neutrality using a dialysis bag; Modified PVA composite film PVA particles and water were stirred at a constant temperature of 95°C for 2 h to prepare a 3% PVA solution, and then an acid-modified nanocellulose suspension was added to the PVA solution at a mass ratio of 1:0.6. Subsequently, vinyltriethoxysilane (KH151) was added to the mixture at 2% of the total mass, and the mixture was stirred at 55°C for 30 min to obtain a membrane solution.

[0025] The experimental group used corona-treated PE as the substrate, coated with modified PVA solution, and prepared into packaging film; the control group also used corona-treated PE as the substrate, coated with unmodified PVA solution as the packaging film. The same batch of yellow peaches with regular morphology and basically the same size were taken to prepare soft-packaged yellow peach products, which were stored at a constant temperature of 25℃ and a relative humidity of 50% for 60 days, and samples were taken on the 0th, 15th, 30th, 45th, 60th, 75th and 90th days to test the changes in the texture characteristics of the bagged yellow peach pulp. The results are shown in Tables 2 and 3.

[0026] Table 2 Experimental groups

[0027] Table 3 Control group

[0028] It is not difficult to find from the data in Tables 2 and 3 that after 90 days of observation, the color of the yellow peach packaged in the packaging film further processed by the nanocellulose (CGF) prepared in Example 1 remained basically unchanged. In sharp contrast, the hardness and chewiness of the yellow peach in the control group decreased significantly in a short period of 45 to 60 days. This result fully verifies the significant effect of the nanocellulose modified PVA material prepared by treating bamboo shoots with a low eutectic solvent in the present invention in improving the performance of the packaging film material, thereby effectively extending the shelf life of the soft-packaged yellow peach.

[0029] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing nanocellulose by treating bamboo shoot shells with a deep eutectic solvent, characterized in that: The steps include: S1. Configuration of deep eutectic solvent: After the first component, the second component and the third component are uniformly mixed, they are stirred and heated to obtain a ternary deep eutectic solvent; S2. Configuration of co-solvent: Benzyltripropylammonium hydroxide, 1'3-bis(hydroxymethyl)urea and water are uniformly mixed, stirred and heated to obtain a cosolvent; S3. Preparation of Nanocellulose: The pretreated bamboo shoot shells, ternary low eutectic solvent and co-solvent are mixed, stirred and heated, and after the reaction is completed, washed with water, filtered and dried to obtain crude cellulose. The crude cellulose is configured into a suspension, ultrasonicated, high-pressure homogenized and freeze-dried to obtain nanocellulose.

2. The method for preparing nanocellulose by treating bamboo shoot shells with a deep eutectic solvent according to claim 1, characterized in that: The first component is choline chloride, the second component is glycerol or oxalic acid, and the third component is any one of aluminum chloride hexahydrate, ferric chloride hexahydrate, and zinc chloride hexahydrate.

3. The method for preparing nanocellulose by treating bamboo shoot shells with a deep eutectic solvent according to claim 1, characterized in that: The molar ratio of the first component, the second component and the third component is 1:1:(0.1-0.3).

4. The method for preparing nanocellulose by treating bamboo shoot shells with a deep eutectic solvent according to claim 1, characterized in that: The mass ratio of the benzyltripropylammonium hydroxide, 1'3-bis(hydroxymethyl)urea and water is 1:1:(10-20).

5. The method for preparing nanocellulose by treating bamboo shoot shells with a deep eutectic solvent according to claim 1, characterized in that: The method of pre-treating bamboo shoot shells is: The bamboo shoot shells were cleaned, dried, cut, and crushed through an 80-mesh sieve to obtain the original sample, referred to as OS; OS was mixed with deionized water in a mass ratio of 1:10, stirred continuously at 90 °C for 2 h, with a rotation speed of 800 rpm, filtered using a 200-mesh sieve, and the solid insoluble matter was placed in an oven and dried at 60 °C for 5 h; The preliminarily treated dry powder was mixed with a 1% NaOH solution at a mass ratio of 1:10, and stirred continuously at 90°C for 2 h at a rotation speed of 800 rpm. After the stirring, it was filtered through a 200-mesh sieve, and the filtered solid was washed with deionized water until the pH of the filtrate was close to neutral. The solid was dried at 60°C for 5 h, and then crushed through an 80-mesh sieve to obtain the pretreated bamboo shoot shell, referred to as PS.

6. The method for preparing nanocellulose by treating bamboo shoot shells with a deep eutectic solvent according to claim 1, characterized in that: The mass ratio of the pretreated bamboo shoot shell, the ternary low eutectic solvent and the co-solvent is (1-10):100:(10-20).

Citation Information

Patent Citations

  • Method utilizing acidosasa edulis bamboo shoot shells to prepare sodium carboxymethylcellulose

    CN104072620A

  • Preparation method of bamboo shoot shell cellulose nano whiskers

    CN112663381A

  • Method for preparing nanocellulose microfibrils through pretreatment of ternary eutectic solvent

    CN112853794A

  • Method for efficiently pretreating corncobs by using ultrasonic-assisted ternary eutectic solvent

    CN114891844A