Green light Micro-LED epitaxial wafer and preparation method thereof
By designing a multi-layer structure and electron injection enhancement layer in the Micro-LED epitaxial sheet, the problem of insufficient light efficiency and yield at low current density in the prior art is solved, and efficient electron hole matching and radiation recombination efficiency are achieved.
Patent Information
- Application Number
- CN202411273538.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The existing Micro-LED epitaxial layer structure design cannot effectively improve the luminous efficiency and yield at low current density, especially the mass of the multi-quantum well luminescent layer and the electron hole concentration matching degree.
A green-light Micro-LED epitaxial sheet is designed, including a substrate, a buffer layer, an N-type semiconductor layer, a low-temperature stress relief layer, a multi-quantum well luminescent layer and an electron barrier layer. The multi-quantum well luminescent layer is made of blue light in front of the well. The well layer, green light multi-quantum well layer and the back-well blue light multi-quantum well layer are composed of the front-well blue light GaN layer, green light GaN layer and back-well blue light GaN layer. The proportion of Al component of the AlGaN barrier layer is Decreasing, and electron injection enhancement layer is added before the multi-quantum well luminescent layer to improve electron hole concentration matching.
The radiation recombination efficiency and electron hole concentration matching of the multi-quantum well luminescent layer are significantly improved, and the luminous efficiency and yield of Micro-LED at low operating current density is improved.
Smart Images

Figure CN118782701B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a green light Micro-LED epitaxial wafer and a preparation method thereof. Background Art
[0002] Micron-sized LED chips (Micro-LED) have excellent properties such as nanosecond-level high-speed response performance, stable characteristics of inorganic materials, high light efficiency, high reliability, high color purity, high contrast, and transparency, and have great application prospects in display, visible light communication, and biomedicine. However, under different current densities, the dominant reasons for the luminescence mechanism of LED devices are different, and the corresponding epitaxial layer structure also changes. For example, in the working range of Micro-LED of 0.01~0.5A / cm 2 At low current density, the carrier concentration in the quantum well is relatively low, the proportion of Auger recombination is small, and the corresponding quantum well recombination volume can be reduced, which can reduce the number of quantum wells, reduce the number of defects, and improve the EQE of the device at low current density; at the same time, electron leakage has not occurred or the proportion is very low at low current density. The electron blocking layer structure not only does not block electrons, but also blocks the injection of holes, reducing the quantum efficiency of the device. The current goal of epitaxial layer structure design and material growth is to improve efficiency at high current density. Its peak EQE is usually in the current density range of 1~4A / cm², but it does not pay attention to the device efficiency at low current density. LEDs designed with traditional epitaxial structures can no longer meet the application requirements of Micro-LEDs. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a green light Micro-LED epitaxial wafer, which can significantly improve the quality of the multi-quantum well light-emitting layer and the matching degree of the electron-hole concentration of the multi-quantum well light-emitting layer, thereby improving the luminous efficiency, yield and other performance of the green light Micro-LED chip at low operating current density.
[0004] The technical problem to be solved by the present invention is also to provide a method for preparing a green light Micro-LED epitaxial wafer, so that the yield of the prepared green light Micro-LED epitaxial wafer is improved and the luminous efficiency is increased at a low operating current density.
[0005] In order to solve the above problems, the present invention provides a green light Micro-LED epitaxial wafer, comprising a substrate, and a buffer layer, an N-type semiconductor layer, a low-temperature stress release layer, a multi-quantum well light-emitting layer, an electron blocking layer and a P-type semiconductor layer sequentially stacked on the substrate;
[0006] The multi-quantum well light-emitting layer comprises a front-well blue light multi-quantum well layer, a green light multi-quantum well layer and a back-well blue light multi-quantum well layer sequentially stacked on the low-temperature stress release layer;
[0007] The pre-well blue light multi-quantum well layer includes a pre-well blue light InGaN layer and a pre-well blue light GaN layer that are periodically and alternately grown, the green light multi-quantum well layer includes a green light InGaN layer and a green light GaN layer that are periodically and alternately grown, and the post-well blue light multi-quantum well layer includes a post-well blue light InGaN layer and a post-well blue light GaN layer that are periodically and alternately grown;
[0008] The proportion of In in the green light InGaN layer is greater than the proportion of In in the blue light InGaN layer before the well and the blue light InGaN layer after the well;
[0009] The pre-well blue light GaN layer, the green light GaN layer and the post-well blue light GaN layer all include a first GaN barrier layer, an AlGaN barrier layer and a second GaN barrier layer stacked in sequence; the Al component ratio of the AlGaN barrier layer in the pre-well blue light GaN layer, the Al component ratio of the AlGaN barrier layer in the green light GaN layer, and the Al component ratio of the AlGaN barrier layer in the post-well blue light GaN layer decrease in sequence.
[0010] As an improvement of the above technical solution, the first GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 0.5nm~2nm; the AlGaN barrier layer is an unintentionally doped AlGaN barrier layer, the Al component ratio is 0.02~0.5, and the thickness is 0.8nm~3.6nm; the second GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 0.5nm~2nm.
[0011] As an improvement of the above technical solution, the Al component ratio of the AlGaN barrier layer in the blue light GaN layer before the well is 0.05-0.5, the Al component ratio of the AlGaN barrier layer in the green light GaN layer is 0.03-0.35, and the Al component ratio of the AlGaN barrier layer in the blue light GaN layer after the well is 0.02-0.25.
[0012] As an improvement of the above technical solution, the growth period of the blue light multi-quantum well layer before the well is 2-6, the blue light InGaN layer before the well is an InGaN layer that is not intentionally doped, the In component ratio is 0.12-0.21, and the thickness is 2.1nm-4.2nm; the blue light GaN layer before the well is a Si-doped GaN layer, and the Si doping concentration is 1.8×10 17 cm -3 ~7.6×10 18 cm -3 , thickness is 7nm~13.8nm;
[0013] The growth period of the green light multi-quantum well layer is 3-8. The green light InGaN layer is an unintentionally doped InGaN layer, the In component ratio is 0.22-0.28, and the thickness is 2.5nm-4.8nm. The green light GaN layer is a Si-doped GaN layer, and the Si doping concentration is 1.2×10 17 cm -3 ~7.5×10 17 cm -3 , thickness is 7nm~13.8nm;
[0014] The growth period of the blue light multi-quantum well layer behind the well is 1-3, the blue light InGaN layer behind the well is an unintentionally doped InGaN layer, the In component ratio is 0.12-0.21, and the thickness is 2.1nm-4.2nm; the blue light GaN layer behind the well is an unintentionally doped GaN layer, and the thickness is 7nm-13.8nm.
[0015] As an improvement of the above technical solution, the multi-quantum well light-emitting layer further includes a first electron injection enhancement layer and a second electron injection enhancement layer, and the first electron injection enhancement layer and the second electron injection enhancement layer are sequentially stacked on the pre-well blue light multi-quantum well layer;
[0016] The first electron injection enhancement layer includes a first electron injection InGaN layer and a first electron injection AlGaN layer that are periodically and alternately grown, and the second electron injection enhancement layer includes a second electron injection InGaN layer and a second electron injection GaN layer that are periodically and alternately grown.
[0017] As an improvement of the above technical solution, the growth period of the first electron injection enhancement layer is 2 to 10, the first electron injection InGaN layer is an unintentionally doped InGaN layer, the In component accounts for 0.03 to 0.12, and the thickness is 0.5 nm to 2.5 nm; the first electron injection AlGaN layer is a Si-doped AlGaN layer, the Al component accounts for 0.02 to 0.25, and the Si doping concentration is 1.65×10 17 cm -3 ~5.2×10 18 cm -3 , thickness is 0.8nm~3nm.
[0018] As an improvement of the above technical solution, the growth period of the second electron injection enhancement layer is 2 to 5; the second electron injection InGaN layer is an unintentionally doped InGaN layer, the In component ratio is 0.01 to 0.08, and the thickness is 0.5 nm to 2.5 nm; the second electron injection GaN layer is a Si-doped GaN layer, and the Si doping concentration is 1.5×10 17 cm -3 ~3.6×1018 cm -3 , thickness is 0.8nm~3nm.
[0019] Correspondingly, the present invention also discloses a method for preparing a green light Micro-LED epitaxial wafer, which is used to prepare the above-mentioned green light Micro-LED epitaxial wafer, comprising the following steps:
[0020] Providing a substrate, and sequentially growing a buffer layer, an N-type semiconductor layer, a low-temperature stress release layer, a multi-quantum well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer on the substrate;
[0021] The multi-quantum well light-emitting layer comprises a pre-well multi-quantum well layer, a green light multi-quantum well layer and a post-well multi-quantum well layer sequentially stacked on the low-temperature stress release layer;
[0022] The pre-well blue light multi-quantum well layer includes a pre-well blue light InGaN layer and a pre-well blue light GaN layer that are periodically and alternately grown, the green light multi-quantum well layer includes a green light InGaN layer and a green light GaN layer that are periodically and alternately grown, and the post-well blue light multi-quantum well layer includes a post-well blue light InGaN layer and a post-well blue light GaN layer that are periodically and alternately grown;
[0023] The proportion of In in the green light InGaN layer is greater than the proportion of In in the blue light InGaN layer before the well and the blue light InGaN layer after the well;
[0024] The pre-well blue light GaN layer, the green light GaN layer and the post-well blue light GaN layer all include a first GaN barrier layer, an AlGaN barrier layer and a second GaN barrier layer stacked in sequence; the Al component ratio of the AlGaN barrier layer in the pre-well blue light GaN layer, the Al component ratio of the AlGaN barrier layer in the green light GaN layer, and the Al component ratio of the AlGaN barrier layer in the post-well blue light GaN layer decrease in sequence.
[0025] As an improvement of the above technical solution, in the pre-well blue light multi-quantum well layer, the growth temperature of the pre-well blue light InGaN layer is 750°C~900°C, and the growth pressure is 50torr~300torr; the growth temperature of the pre-well blue light GaN layer is 830°C~920°C, and the growth pressure is 50torr~300torr;
[0026] In the green multi-quantum well layer, the growth temperature of the green InGaN layer is 706°C to 890°C, and the growth pressure is 50torr to 300torr; the growth temperature of the green GaN layer is 830°C to 920°C, and the growth pressure is 50torr to 300torr;
[0027] In the back-well blue light multi-quantum well layer, the growth temperature of the back-well blue light InGaN layer is 750° C. to 900° C., and the growth pressure is 50 torr to 300 torr; the growth temperature of the back-well blue light GaN layer is 830° C. to 920° C., and the growth pressure is 50 torr to 300 torr;
[0028] The pre-well blue light GaN layer, the green light GaN layer and the post-well blue light GaN layer all include a first GaN barrier layer, an AlGaN barrier layer and a second GaN barrier layer stacked in sequence, wherein the growth temperature of the first GaN barrier layer is 800°C~920°C, and the growth pressure is 50torr~300torr, the growth temperature of the AlGaN barrier layer is 800°C~920°C, and the growth pressure is 50torr~300torr, and the growth temperature of the second GaN barrier layer is 800°C~920°C, and the growth pressure is 50torr~300torr.
[0029] As an improvement of the above technical solution, it also includes sequentially growing a first electron injection enhancement layer and a second electron injection enhancement layer on the pre-well blue light multi-quantum well layer; the first electron injection enhancement layer includes a first electron injection InGaN layer and a first electron injection AlGaN layer that are periodically and alternately grown, and the second electron injection enhancement layer includes a second electron injection InGaN layer and a second electron injection GaN layer that are periodically and alternately grown;
[0030] In the first electron injection enhancement layer, the growth temperature of the first electron injection InGaN layer is 780°C to 890°C, and the growth pressure is 50torr to 300torr; the growth temperature of the first electron injection AlGaN layer is 780°C to 890°C, and the growth pressure is 50torr to 300torr;
[0031] In the second electron injection enhancement layer, the growth temperature of the second electron injection InGaN layer is 780°C~890°C, and the growth pressure is 50torr~300torr; the growth temperature of the second electron injection GaN layer is 780°C~890°C, and the growth pressure is 50torr~300torr.
[0032] The implementation of the present invention has the following beneficial effects:
[0033] 1. The multi-quantum well light-emitting layer of the present invention comprises a blue light multi-quantum well layer before the well, a green light multi-quantum well layer and a blue light multi-quantum well layer after the well, wherein the In component in the blue light InGaN layer before the well, the green light InGaN layer and the blue light InGaN layer after the well is first increased and then decreased, which can effectively improve the quality of the green light multi-quantum well layer, thereby improving the radiation recombination efficiency of the multi-quantum well light-emitting layer; in addition, the blue light GaN layer before the well, the green light GaN layer and the blue light GaN layer after the well all comprise a first GaN barrier layer, an AlGaN barrier layer and a second GaN barrier layer stacked in sequence, and the blue light GaN layer before the well is The Al component ratio of the AlGaN barrier layer in the GaN layer, the Al component ratio of the AlGaN barrier layer in the green light GaN layer, and the Al component ratio of the AlGaN barrier layer in the blue light GaN layer behind the well decreases gradually, which can effectively bind electrons in front of the green light multi-quantum well region, blocking electrons and reducing the electron movement rate, thereby improving the matching degree of the electron-hole concentration in the multi-quantum well light-emitting layer, improving the luminous efficiency of the Micro-LED at low operating current density, and preventing electrons from being injected into the P-type semiconductor layer to cause electron leakage, thereby improving the yield rate of the green light Micro-LED and other performance.
[0034] 2. The present invention is designed with a first electron injection enhancement layer and a second electron injection enhancement layer before the green light multi-quantum well layer. The low-barrier InGaN material in the first electron injection enhancement layer and the second electron injection enhancement layer can store part of the electrons, significantly improving the matching degree of the electron-hole concentration in the green light multi-quantum well layer, thereby improving the luminous efficiency of the green light Micro-LED chip at low operating current density. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is a schematic structural diagram of a green light Micro-LED epitaxial wafer in an embodiment of the present invention;
[0036] Figure 2 is a schematic diagram of the structure of a multi-quantum well light-emitting layer of a green light Micro-LED epitaxial wafer in an embodiment of the present invention;
[0037] Figure 3 is a schematic structural diagram of a multi-quantum well light-emitting layer of a green light Micro-LED epitaxial wafer in another embodiment of the present invention;
[0038] Figure 4 It is a flow chart of the method for preparing a green light Micro-LED epitaxial wafer in an embodiment of the present invention. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below in conjunction with specific embodiments.
[0040] like Figure 1 and Figure 2As shown, an embodiment of the present invention provides a green light Micro-LED epitaxial wafer, including a substrate 100, and a buffer layer 200, an N-type semiconductor layer 300, a low-temperature stress release layer 400, a multi-quantum well light-emitting layer 500, an electron blocking layer 600 and a P-type semiconductor layer 700 sequentially stacked on the substrate 100.
[0041] The multi-quantum well light emitting layer 500 includes a front-well blue multi-quantum well layer 510 , a green multi-quantum well layer 540 , and a back-well blue multi-quantum well layer 550 , which are sequentially stacked on the low-temperature stress release layer 400 .
[0042] Specifically, the pre-well blue light multi-quantum well layer 510 is a periodic structure, and each period includes a pre-well blue light InGaN layer and a pre-well blue light GaN layer; the green light multi-quantum well layer 540 is a periodic structure, and each period includes a green light InGaN layer and a green light GaN layer; the post-well blue light multi-quantum well layer 550 is a periodic structure, and each period includes a post-well blue light InGaN layer and a post-well blue light GaN layer, and the proportion of In component in the green light InGaN layer is greater than the proportion of In component in the pre-well blue light InGaN layer and the post-well blue light InGaN layer, and the In component in the pre-well blue light InGaN layer, the green light InGaN layer and the post-well blue light InGaN layer first increases and then decreases, which can effectively improve the quality of the green light multi-quantum well layer, thereby improving the radiation recombination efficiency of the active region.
[0043] In addition, the blue light GaN layer before the well, the green light GaN layer and the blue light GaN layer after the well all include a first GaN barrier layer, an AlGaN barrier layer and a second GaN barrier layer stacked in sequence, which play a role in blocking electrons and reducing the electron movement rate, thereby improving the matching degree of the electron-hole concentration of the multi-quantum well light-emitting layer.
[0044] In one embodiment, the first GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 0.5nm~2nm, exemplarily 0.8nm, 1nm, 1.2nm, 1.5nm or 1.8nm, but not limited thereto. The AlGaN barrier layer is an unintentionally doped AlGaN barrier layer, and the Al component ratio is 0.02~0.5, exemplarily 0.06, 0.1, 0.2, 0.3 or 0.4, but not limited thereto. The thickness of the AlGaN barrier layer is 0.8nm~3.6nm, exemplarily 1nm, 2nm, 2.5nm, 3nm or 3.5nm, but not limited thereto. The second GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 0.5nm~2nm, exemplarily 0.8nm, 1nm, 1.2nm, 1.5nm or 1.8nm, but not limited thereto.
[0045] In a preferred embodiment, the Al component ratio of the AlGaN barrier layer in the blue light GaN layer before the well, the Al component ratio of the AlGaN barrier layer in the green light GaN layer, and the Al component ratio of the AlGaN barrier layer in the blue light GaN layer after the well decrease successively, which can effectively bind electrons in front of the green light multi-quantum well region, play a role in blocking electrons and reducing the electron movement rate, thereby improving the matching degree of the electron-hole concentration of the multi-quantum well light-emitting layer, improving the luminous efficiency of the Micro-LED at low operating current density, and preventing electrons from being injected into the P-type semiconductor layer to cause electron leakage, thereby improving the yield rate of the green light Micro-LED and other performance.
[0046] Specifically, the Al component ratio of the AlGaN barrier layer in the blue light GaN layer before the well is 0.05-0.5, the Al component ratio of the AlGaN barrier layer in the green light GaN layer is 0.03-0.35, and the Al component ratio of the AlGaN barrier layer in the blue light GaN layer after the well is 0.02-0.25.
[0047] In one embodiment, the growth period of the pre-well blue light multi-quantum well layer 510 is 2 to 6, the pre-well blue light InGaN layer is an unintentionally doped InGaN single layer or multilayer structure, and the In component ratio is 0.12 to 0.21, and is 0.13, 0.15, 0.16, 0.18 or 0.2, but not limited to this. The thickness of the pre-well blue light InGaN layer is 2.1nm to 4.2nm, and is 2.5nm, 3nm, 3.5nm, 3.8nm or 4nm, but not limited to this. The pre-well blue light GaN layer is a Si-doped GaN single layer or multilayer structure, and the Si doping concentration is 1.8×10 17 cm -3 ~7.6×10 18 cm -3 , exemplarily 2×10 17 cm -3 , 5×10 17 cm -3 , 8×10 17 cm -3 , 1×10 18 cm -3 or 5×10 18 cm -3 The thickness of the pre-well blue light GaN layer is 7 nm to 13.8 nm, and is exemplarily 8 nm, 9 nm, 10 nm, 11 nm or 12 nm, but is not limited thereto.
[0048] In one embodiment, the growth period of the green light multi-quantum well layer 540 is 3 to 8, the green light InGaN layer is an InGaN single layer or multilayer structure that is not intentionally doped, and the In component ratio is 0.22 to 0.28, and is 0.23, 0.24, 0.25, 0.26 or 0.27, but not limited thereto. The thickness of the green light InGaN layer is 2.5 nm to 4.8 nm, and is 2.8 nm, 3 nm, 3.5 nm, 4 nm or 4.5 nm, but not limited thereto. The green light GaN layer is a Si-doped GaN single layer or multilayer structure, and the Si doping concentration is 1.2×10 17 cm -3 ~7.5×10 17 cm -3 , exemplarily 2×10 17 cm -3 , 2.5×10 17 cm -3 , 4×10 17 cm -3 , 5×10 17 cm -3 or 6×10 17 cm -3 The thickness of the green light GaN layer is 7 nm to 13.8 nm, and is exemplarily 8 nm, 9 nm, 10 nm, 11 nm or 12 nm, but is not limited thereto.
[0049] In one embodiment, the growth period of the post-well blue light multi-quantum well layer 550 is 1 to 3, the post-well blue light InGaN layer is an unintentionally doped InGaN single layer or multilayer structure, and the In component ratio is 0.12 to 0.21, and is 0.13, 0.14, 0.15, 0.16 or 0.18, but not limited thereto. The thickness of the post-well blue light InGaN layer is 2.1 nm to 4.2 nm, and is 2.5 nm, 3 nm, 3.2 nm, 3.5 nm or 4 nm, but not limited thereto. The post-well blue light GaN layer is an unintentionally doped GaN single layer or multilayer structure, and has a thickness of 7 nm to 13.8 nm, and is 8 nm, 9 nm, 10 nm, 11 nm or 12 nm, but not limited thereto.
[0050] like Figure 3As shown, in a preferred embodiment, the multi-quantum well light-emitting layer 500 further includes a first electron injection enhancement layer 520 and a second electron injection enhancement layer 530, and the first electron injection enhancement layer 520 and the second electron injection enhancement layer 530 are sequentially stacked on the pre-well blue light multi-quantum well layer 510. The first electron injection enhancement layer 520 includes a first electron injection InGaN layer and a first electron injection AlGaN layer that are periodically and alternately grown, and the second electron injection enhancement layer 530 includes a second electron injection InGaN layer and a second electron injection GaN layer that are periodically and alternately grown. The low-barrier InGaN material in the first electron injection enhancement layer 520 and the second electron injection enhancement layer 530 can store part of the electrons, significantly improving the matching degree of the electron-hole concentration in the green light multi-quantum well layer, thereby improving the light efficiency of the green light Micro-LED chip at a low operating current density.
[0051] In one embodiment, the growth period of the first electron injection enhancement layer 520 is 2 to 10, the first electron injection InGaN layer is an unintentionally doped InGaN layer, and the In component ratio is 0.03 to 0.12, and is 0.05, 0.07, 0.08, 0.09 or 0.1, but not limited to this. The thickness of the first electron injection InGaN layer is 0.5nm to 2.5nm, and is 0.8nm, 1nm, 1.5nm, 1.8nm or 2nm, but not limited to this. The first electron injection AlGaN layer is a Si-doped AlGaN layer, and the Al component ratio is 0.02 to 0.25, and is 0.05, 0.08, 0.1, 0.15 or 0.2, but not limited to this. The Si doping concentration of the first electron injection AlGaN layer is 1.65×10 17 cm -3 ~5.2×10 18 cm -3 , exemplarily 2×10 17 cm -3 , 5×10 17 cm -3 , 8×10 17 cm -3 , 1×10 18 cm -3 or 2.5 × 10 18 cm -3 The thickness of the first electron injection AlGaN layer is 0.8 nm to 3 nm, and is exemplarily 1 nm, 1.5 nm, 2 nm, 2.5 nm or 2.8 nm, but is not limited thereto.
[0052] In one embodiment, the growth period of the second electron injection enhancement layer 530 is 2 to 5, the second electron injection InGaN layer is an unintentionally doped InGaN layer, and the In component ratio is 0.01 to 0.08, and is 0.02, 0.04, 0.05, 0.06 or 0.08, but not limited thereto. The thickness of the second electron injection InGaN layer is 0.5 nm to 2.5 nm, and is 0.8 nm, 1 nm, 1.5 nm, 1.8 nm or 2 nm, but not limited thereto. The second electron injection GaN layer is a Si-doped GaN layer, and the Si doping concentration is 1.5×10 17 cm -3 ~3.6×10 18 cm -3 , exemplarily 2×10 17 cm -3 , 5×10 17 cm -3 , 8×10 17 cm -3 , 1×10 18 cm -3 or 2.5 × 10 18 cm -3 The thickness of the second electron injection GaN layer is 0.8 nm to 3 nm, and is exemplarily 1 nm, 1.5 nm, 2 nm, 2.5 nm or 2.8 nm, but is not limited thereto.
[0053] In addition to the above-mentioned multi-quantum well light-emitting layer structure, the other layered structures of the present invention are characterized as follows:
[0054] The substrate 100 can be selected from one of sapphire substrate, SiO2 sapphire composite substrate, silicon substrate, silicon carbide substrate, gallium nitride substrate, and zinc oxide substrate. Specifically, the substrate 100 is selected from sapphire substrate, which is currently the most commonly used GaN-based LED substrate material. Sapphire substrate has the advantages of mature preparation technology, low price, easy cleaning and processing, and good stability at high temperature.
[0055] The buffer layer 200 may be one or more of an AlN buffer layer, an AlGaN buffer layer, and a GaN buffer layer. Specifically, the buffer layer 200 uses an AlN buffer layer with a thickness of 10nm to 50nm. The AlN buffer layer provides a nucleation center with the same orientation as the substrate, releases the stress generated by the lattice mismatch between GaN and the substrate and the thermal stress generated by the mismatch of thermal expansion coefficients, provides a flat nucleation surface for further growth, reduces the contact angle of its nucleation growth, and enables the island-like growth of GaN grains to be connected to a surface within a smaller thickness, thus transforming into two-dimensional epitaxial growth.
[0056] The N-type semiconductor layer 300 includes an undoped GaN layer and an N-type GaN layer. The thickness of the undoped GaN layer is 1 μm to 5 μm, the thickness of the N-type GaN layer is 2 μm to 3 μm, and the Si doping concentration is 1×10 19 cm -3 ~5×10 19 cm -3 .
[0057] The low temperature stress release layer 400 may be an InGaN / GaN periodic structure with a growth period of 2 to 10, wherein the thickness of the InGaN layer is 1 nm to 3 nm, and the thickness of the GaN layer is 15 nm to 30 nm. The growth temperature of the low temperature stress release layer 400 is 800° C. to 900° C., and the growth pressure is 100 torr to 500 torr.
[0058] The electron blocking layer 600 may be an AlInGaN electron blocking layer with a thickness of 10 nm to 40 nm, an Al component ratio of 0.005 to 0.1, and an In component ratio of 0.01 to 0.2. This layer can effectively limit electron overflow, reduce the blocking of holes, improve the injection efficiency of holes into quantum wells, reduce carrier Auger recombination, and improve the luminous efficiency of the LED.
[0059] The P-type semiconductor layer 700 may be a P-type GaN layer with a thickness of 10 nm to 50 nm and a Mg doping concentration of 1×10 19 cm -3 ~1×10 21 cm -3 , too high Mg doping concentration will destroy the crystal quality, while too low doping concentration will affect the hole concentration.
[0060] like Figure 4 As shown, the present invention also discloses a method for preparing a green light Micro-LED epitaxial wafer, comprising the following steps:
[0061] S1. Provide a substrate.
[0062] S2. A buffer layer, an N-type semiconductor layer, a low-temperature stress release layer, a multi-quantum well light-emitting layer, an electron blocking layer and a P-type semiconductor layer are sequentially grown on the substrate, wherein the multi-quantum well light-emitting layer comprises a front-well blue light multi-quantum well layer, a green light multi-quantum well layer and a back-well blue light multi-quantum well layer sequentially stacked on the low-temperature stress release layer.
[0063] Specifically, the preparation of the pre-well blue light multi-quantum well layer includes the following steps:
[0064] The temperature of the reaction chamber is controlled at 750°C~900°C and the pressure is 50torr~300torr, and N source, Ga source and In source are introduced to grow a front-well blue light InGaN layer; the temperature of the reaction chamber is controlled at 830°C~920°C and the pressure is 50torr~300torr, and N source, Ga source and Si source are introduced to grow a front-well blue light GaN layer; the front-well blue light InGaN layer and the front-well blue light GaN layer are repeatedly stacked to periodically grow.
[0065] In one embodiment, the preparation of the pre-well blue light GaN layer further comprises the following steps:
[0066] After growing the front-well blue light GaN layer, control the temperature of the reaction chamber to 800°C~920°C and the pressure to 50torr~300torr, introduce N source and Ga source to grow the first GaN barrier layer; control the temperature of the reaction chamber to 800°C~920°C and the pressure to 50torr~300torr, grow the AlGaN barrier layer; control the temperature of the reaction chamber to 800°C~920°C and the pressure to 50torr~300torr, grow the second GaN barrier layer, and continue to grow the front-well blue light GaN layer.
[0067] The preparation of the green light multi-quantum well layer comprises the following steps:
[0068] The temperature of the reaction chamber is controlled at 706°C~890°C and the pressure is 50torr~300torr, and N source, Ga source and In source are introduced to grow a green light InGaN layer; the temperature of the reaction chamber is controlled at 830°C~920°C and the pressure is 50torr~300torr, and N source, Ga source and Si source are introduced to grow a green light GaN layer; the green light InGaN layer and the green light GaN layer are repeatedly stacked to grow periodically.
[0069] In one embodiment, the preparation of the green light GaN layer further comprises the following steps:
[0070] After growing the green light GaN layer, the reaction chamber temperature is controlled to be 800°C~920°C and the pressure is 50torr~300torr, and the N source and Ga source are introduced to grow the first GaN barrier layer; the reaction chamber temperature is controlled to be 800°C~920°C and the pressure is 50torr~300torr, and the AlGaN barrier layer is grown; the reaction chamber temperature is controlled to be 800°C~920°C and the pressure is 50torr~300torr, and the second GaN barrier layer is grown, and the green light GaN layer continues to grow.
[0071] The preparation of the back-well blue light multi-quantum well layer comprises the following steps:
[0072] The temperature of the reaction chamber is controlled at 750°C~900°C and the pressure is 50torr~300torr, and N source, Ga source and In source are introduced to grow a blue light InGaN layer behind the well; the temperature of the reaction chamber is controlled at 830°C~920°C and the pressure is 50torr~300torr to grow a blue light GaN layer behind the well; and the blue light InGaN layer behind the well and the blue light GaN layer behind the well are repeatedly stacked to periodically grow.
[0073] In one embodiment, the preparation of the post-well blue light GaN layer further comprises the following steps:
[0074] After growing the blue light GaN layer behind the well, control the temperature of the reaction chamber to 800℃~920℃ and the pressure to 50torr~300torr, introduce N source and Ga source to grow the first GaN barrier layer; control the temperature of the reaction chamber to 800℃~920℃ and the pressure to 50torr~300torr, grow the AlGaN barrier layer; control the temperature of the reaction chamber to 800℃~920℃ and the pressure to 50torr~300torr, grow the second GaN barrier layer, and continue to grow the blue light GaN layer behind the well.
[0075] The growth temperature of InGaN material in the pre-well blue multi-quantum well layer and the post-well blue multi-quantum well layer is higher than that of InGaN material in the green multi-quantum well layer. InGaN material is grown at high temperature, has high atomic mobility, and is more inclined to grow two-dimensional materials. The defects in the InGaN material will be significantly reduced, and it is easier to obtain high-quality InGaN material. At the same time, the In component ratio of InGaN material in the pre-well blue multi-quantum well layer and the post-well blue multi-quantum well layer is lower than that of InGaN material in the green multi-quantum well layer. The lattice mismatch stress between the InGaN material and the GaN material in the green multi-quantum well layer is reduced, and the defects caused by large mismatch stress are reduced, which can significantly improve the quality of the multi-quantum well light-emitting layer. The reduction of defects in the multi-quantum well light-emitting layer is beneficial to improving the radiation recombination efficiency of the active region, thereby improving the luminous efficiency and yield of the green light Micro-LED at low operating current density.
[0076] In a preferred embodiment, the invention further comprises: growing a first electron injection enhancement layer and a second electron injection enhancement layer on the pre-well blue light multi-quantum well layer.
[0077] Specifically, the preparation of the first electron injection enhancement layer includes the following steps:
[0078] The temperature of the reaction chamber is controlled at 780°C to 890°C and the pressure is 50 torr to 300 torr, and N source, Ga source and In source are introduced to grow a first electron injection InGaN layer; the temperature of the reaction chamber is controlled at 780°C to 890°C and the pressure is 50 torr to 300 torr, and N source, Ga source, Al source and Si source are introduced to grow a first electron injection AlGaN layer; the first electron injection InGaN layer and the first electron injection AlGaN layer are repeatedly stacked to periodically grow.
[0079] The preparation of the second electron injection enhancement layer comprises the following steps:
[0080] The temperature of the reaction chamber is controlled at 780°C to 890°C and the pressure is 50 torr to 300 torr, and an N source, a Ga source and an In source are introduced to grow a second electron injection InGaN layer; the temperature of the reaction chamber is controlled at 780°C to 890°C and the pressure is 50 torr to 300 torr, and an N source, a Ga source and a Si source are introduced to grow a second electron injection GaN layer; and the second electron injection InGaN layer and the second electron injection GaN layer are repeatedly stacked to periodically grow.
[0081] The present invention is further described below with reference to specific embodiments.
[0082] Example 1
[0083] The present embodiment provides a green light Micro-LED epitaxial wafer, including a substrate and a buffer layer, an N-type semiconductor layer, a low-temperature stress release layer, a multi-quantum well light-emitting layer, an electron blocking layer and a P-type semiconductor layer stacked in sequence on the substrate, and the multi-quantum well light-emitting layer includes a pre-well blue light multi-quantum well layer, a green light multi-quantum well layer and a post-well blue light multi-quantum well layer stacked in sequence on the low-temperature stress release layer.
[0084] The pre-well blue light multi-quantum well layer includes a pre-well blue light InGaN layer and a pre-well blue light GaN layer that are grown periodically and alternately. The number of periods is 5. The pre-well blue light InGaN layer is an unintentionally doped InGaN layer, with an In component ratio of 0.15 and a thickness of 3nm. The pre-well blue light GaN layer is a Si-doped GaN layer with a Si doping concentration of 5×10 17 cm -3 , with a thickness of 7.5nm. The first GaN barrier layer, the AlGaN barrier layer and the second GaN barrier layer are also inserted in the blue light GaN layer before the well. The first GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 0.8nm; the AlGaN barrier layer is an unintentionally doped AlGaN barrier layer with an Al component ratio of 0.4 and a thickness of 2nm; the second GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 1.2nm.
[0085] The green multi-quantum well layer includes a green InGaN layer and a green GaN layer that are grown periodically and alternately. The number of periods is 5. The green InGaN layer is an unintentionally doped InGaN layer, with an In component ratio of 0.25 and a thickness of 3nm. The green GaN layer is a Si-doped GaN layer with a Si doping concentration of 5×10 17 cm -3 , with a thickness of 7.5nm. The first GaN barrier layer, the AlGaN barrier layer and the second GaN barrier layer are also inserted in the green light GaN layer. The first GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 0.8nm; the AlGaN barrier layer is an unintentionally doped AlGaN barrier layer with an Al component ratio of 0.2 and a thickness of 2nm; the second GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 1.2nm.
[0086] The blue light multi-quantum well layer behind the well includes a blue light InGaN layer behind the well and a blue light GaN layer behind the well that are grown periodically and alternately, with a period number of 2. The blue light InGaN layer behind the well is an unintentionally doped InGaN layer, with an In component ratio of 0.15 and a thickness of 3nm. The blue light GaN layer behind the well is an unintentionally doped GaN layer with a thickness of 7.5nm. The first GaN barrier layer, the AlGaN barrier layer and the second GaN barrier layer are also inserted into the blue light GaN layer behind the well. The first GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 0.8nm; the AlGaN barrier layer is an unintentionally doped AlGaN barrier layer with an Al component ratio of 0.1 and a thickness of 2nm; the second GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 1.2nm.
[0087] The method for preparing the green light Micro-LED epitaxial wafer comprises the following steps:
[0088] S100 A substrate is provided.
[0089] S200 A buffer layer, an N-type semiconductor layer, a low-temperature stress release layer, a multi-quantum well light-emitting layer, an electron blocking layer and a P-type semiconductor layer are sequentially grown on the substrate, wherein the multi-quantum well light-emitting layer comprises a front-well blue light multi-quantum well layer, a green light multi-quantum well layer and a back-well blue light multi-quantum well layer sequentially stacked on the low-temperature stress release layer.
[0090] Specifically, the preparation of the pre-well blue light multi-quantum well layer includes the following steps:
[0091] The temperature of the reaction chamber is controlled at 780°C and the pressure is 120 torr, and N source, Ga source and In source are introduced to grow a blue light InGaN layer in front of the well; the temperature of the reaction chamber is controlled at 880°C and the pressure is 120 torr, and N source, Ga source and Si source are introduced to grow a blue light GaN layer in front of the well; the blue light InGaN layer in front of the well and the blue light GaN layer in front of the well are repeatedly stacked to periodically grow.
[0092] The preparation of the blue light GaN layer before the well also includes the following steps:
[0093] After growing the blue light GaN layer in front of the well, the reaction chamber temperature is controlled at 850°C and the pressure is 120 torr, and the N source and Ga source are introduced to grow the first GaN barrier layer; the reaction chamber temperature is controlled at 850°C and the pressure is 120 torr to grow the AlGaN barrier layer; the reaction chamber temperature is controlled at 880°C and the pressure is 120 torr to grow the second GaN barrier layer, and the growth of the blue light GaN layer in front of the well continues.
[0094] The preparation of the green light multi-quantum well layer includes the following steps:
[0095] The temperature of the reaction chamber is controlled at 780°C and the pressure is 120 torr, and N source, Ga source and In source are introduced to grow a green light InGaN layer; the temperature of the reaction chamber is controlled at 850°C and the pressure is 120 torr, and N source, Ga source and Si source are introduced to grow a green light GaN layer; the green light InGaN layer and the green light GaN layer are repeatedly stacked to grow periodically.
[0096] The preparation of the green light GaN layer also includes the following steps:
[0097] After growing the green light GaN layer, the reaction chamber temperature is controlled at 850°C and the pressure is 120 torr, and the N source and Ga source are introduced to grow the first GaN barrier layer; the reaction chamber temperature is controlled at 850°C and the pressure is 120 torr to grow the AlGaN barrier layer; the reaction chamber temperature is controlled at 880°C and the pressure is 120 torr to grow the second GaN barrier layer, and the green light GaN layer continues to grow.
[0098] The preparation of the back-well blue light multi-quantum well layer includes the following steps:
[0099] The temperature of the reaction chamber is controlled at 790°C and the pressure is 120 torr, and N source, Ga source and In source are introduced to grow a blue light InGaN layer behind the well; the temperature of the reaction chamber is controlled at 880°C and the pressure is 120 torr, and N source and Ga source are introduced to grow a blue light GaN layer behind the well; the blue light InGaN layer behind the well and the blue light GaN layer behind the well are repeatedly stacked to periodically grow.
[0100] The preparation of the blue light GaN layer behind the well also includes the following steps:
[0101] After growing the blue light GaN layer behind the well, the reaction chamber temperature is controlled at 850°C and the pressure is 120 torr, and the N source and Ga source are introduced to grow the first GaN barrier layer; the reaction chamber temperature is controlled at 850°C and the pressure is 120 torr to grow the AlGaN barrier layer; the reaction chamber temperature is controlled at 880°C and the pressure is 120 torr to grow the second GaN barrier layer, and the growth of the blue light GaN layer behind the well is continued.
[0102] Example 2
[0103] This embodiment provides a green light Micro-LED epitaxial wafer, which is different from the embodiment 1 in that the multi-quantum well light-emitting layer also includes a first electron injection enhancement layer and a second electron injection enhancement layer, and the first electron injection enhancement layer and the second electron injection enhancement layer are sequentially stacked on the pre-well blue light multi-quantum well layer. The first electron injection enhancement layer includes a first electron injection InGaN layer and a first electron injection AlGaN layer that are periodically and alternately grown, with a growth period of 6. The first electron injection InGaN layer is an unintentionally doped InGaN layer, with an In component ratio of 0.06 and a thickness of 1.5nm; the first electron injection AlGaN layer is a Si-doped AlGaN layer, with an Al component ratio of 0.12 and a Si doping concentration of 5×10 17 cm -3 , with a thickness of 2.5nm. The second electron injection enhancement layer includes a second electron injection InGaN layer and a second electron injection GaN layer that are periodically and alternately grown, with a growth period of 3. The second electron injection InGaN layer is an unintentionally doped InGaN layer, with an In component ratio of 0.04 and a thickness of 1.5nm; the second electron injection GaN layer is a Si-doped GaN layer, with a Si doping concentration of 6×10 17 cm -3 , with a thickness of 2nm.
[0104] Correspondingly, the method for preparing the multi-quantum well light-emitting layer also includes:
[0105] Growing a first electron injection enhancement layer on the pre-well blue light multi-quantum well layer comprises the following steps:
[0106] The temperature of the reaction chamber is controlled at 820°C and the pressure is 120 torr, and N source, Ga source and In source are introduced to grow a first electron injection InGaN layer; the temperature of the reaction chamber is controlled at 850°C and the pressure is 120 torr, and N source, Ga source, Al source and Si source are introduced to grow a first electron injection AlGaN layer; the first electron injection InGaN layer and the first electron injection AlGaN layer are repeatedly stacked to periodically grow.
[0107] Growing a second electron injection enhancement layer on the first electron injection enhancement layer comprises the following steps:
[0108] The temperature of the reaction chamber is controlled at 810°C and the pressure is 120 torr, and N source, Ga source and In source are introduced to grow a second electron injection InGaN layer; the temperature of the reaction chamber is controlled at 850°C and the pressure is 120 torr, and N source, Ga source and Si source are introduced to grow a second electron injection GaN layer; the second electron injection InGaN layer and the second electron injection GaN layer are repeatedly stacked to periodically grow.
[0109] The rest are the same as in Example 1.
[0110] Comparative Example 1
[0111] This comparative example provides a green light Micro-LED epitaxial wafer, which is different from Example 1 in that the multi-quantum well light-emitting layer is a green multi-quantum well layer. Accordingly, the preparation method does not include the preparation of the pre-well blue multi-quantum well layer and the post-well blue multi-quantum well layer.
[0112] The rest are the same as in Example 1.
[0113] Comparative Example 2
[0114] This comparative example provides a green light Micro-LED epitaxial wafer, which is different from Example 1 in that the multi-quantum well light-emitting layer is a pre-well blue light multi-quantum well layer and a green light multi-quantum well layer stacked in sequence. Accordingly, the preparation method does not include the preparation of the post-well blue light multi-quantum well layer.
[0115] The rest are the same as in Example 1.
[0116] Comparative Example 3
[0117] This comparative example provides a green light Micro-LED epitaxial wafer, which is different from Example 1 in that the multi-quantum well light-emitting layer is a green light multi-quantum well layer and a back-well blue light multi-quantum well layer stacked in sequence. Accordingly, the preparation method does not include the preparation of the front-well blue light multi-quantum well layer.
[0118] The rest are the same as in Example 1.
[0119] Comparative Example 4
[0120] This comparative example provides a green light Micro-LED epitaxial wafer, which is different from Example 1 in that the blue light GaN layer before the well is a Si-doped GaN layer with a Si doping concentration of 5×10 17 cm -3 , with a thickness of 7.5nm; the green light GaN layer is a Si-doped GaN layer with a Si doping concentration of 5×10 17 cm -3 , with a thickness of 7.5nm; the blue light GaN layer behind the well is a GaN layer that is not intentionally doped, with a thickness of 7.5nm.
[0121] Accordingly, the preparation method does not include the preparation of the first GaN barrier layer, the AlGaN barrier layer and the second GaN barrier layer.
[0122] The rest are the same as in Example 1.
[0123] Performance Test:
[0124] The green Micro-LED epitaxial wafers prepared in Example 1, Example 2, and Comparative Examples 1 to 4 were made into 20μm×20μm green Micro-LED chips, which were tested on the same LED spot tester at a current of 0.5μA / 3μA / 10μA, and the luminous efficiency improvement of Example 1, Example 2, and Comparative Examples 2 to 4 compared to Comparative Example 1 was calculated.
[0125] The test results are shown in Table 1.
[0126] Table 1 Photoelectric performance test results of green light Micro-LED
[0127]
[0128] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.
Claims
1. A green light Micro-LED epitaxial wafer, characterized in that: It includes a substrate, and a buffer layer, an N-type semiconductor layer, a low-temperature stress release layer, a multi-quantum well light-emitting layer, an electron blocking layer and a P-type semiconductor layer sequentially stacked on the substrate; The multi-quantum well light-emitting layer comprises a front-well blue light multi-quantum well layer, a green light multi-quantum well layer and a back-well blue light multi-quantum well layer sequentially stacked on the low-temperature stress release layer; The pre-well blue light multi-quantum well layer includes a pre-well blue light InGaN layer and a pre-well blue light GaN layer that are periodically and alternately grown, the green light multi-quantum well layer includes a green light InGaN layer and a green light GaN layer that are periodically and alternately grown, and the post-well blue light multi-quantum well layer includes a post-well blue light InGaN layer and a post-well blue light GaN layer that are periodically and alternately grown; The proportion of In in the green light InGaN layer is greater than the proportion of In in the blue light InGaN layer before the well and the blue light InGaN layer after the well; The pre-well blue light GaN layer, the green light GaN layer and the post-well blue light GaN layer all include a first GaN barrier layer, an AlGaN barrier layer and a second GaN barrier layer stacked in sequence; the Al component ratio of the AlGaN barrier layer in the pre-well blue light GaN layer, the Al component ratio of the AlGaN barrier layer in the green light GaN layer, and the Al component ratio of the AlGaN barrier layer in the post-well blue light GaN layer decrease in sequence.
2. The green light Micro-LED epitaxial wafer according to claim 1, characterized in that: The first GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 0.5nm~2nm; the AlGaN barrier layer is an unintentionally doped AlGaN barrier layer with an Al component ratio of 0.02~0.5 and a thickness of 0.8nm~3.6nm; the second GaN barrier layer is an unintentionally doped GaN barrier layer with a thickness of 0.5nm~2nm.
3. The green light Micro-LED epitaxial wafer according to claim 2, characterized in that: The Al component ratio of the AlGaN barrier layer in the blue light GaN layer before the well is 0.05-0.5, the Al component ratio of the AlGaN barrier layer in the green light GaN layer is 0.03-0.35, and the Al component ratio of the AlGaN barrier layer in the blue light GaN layer after the well is 0.02-0.
25.
4. The green light Micro-LED epitaxial wafer according to claim 1, characterized in that: The growth period of the blue light multi-quantum well layer before the well is 2-6. The blue light InGaN layer before the well is an unintentionally doped InGaN layer, the In component ratio is 0.12-0.21, and the thickness is 2.1nm-4.2nm. The blue light GaN layer before the well is a Si-doped GaN layer, and the Si doping concentration is 1.8×10 17 cm -3 ~7.6×10 18 cm -3 , thickness is 7nm~13.8nm; The growth period of the green light multi-quantum well layer is 3-8. The green light InGaN layer is an unintentionally doped InGaN layer, the In component ratio is 0.22-0.28, and the thickness is 2.5nm-4.8nm. The green light GaN layer is a Si-doped GaN layer, and the Si doping concentration is 1.2×10 17 cm -3 ~7.5×10 17 cm -3 , thickness is 7nm~13.8nm; The growth period of the blue light multi-quantum well layer behind the well is 1-3, the blue light InGaN layer behind the well is an unintentionally doped InGaN layer, the In component ratio is 0.12-0.21, and the thickness is 2.1nm-4.2nm; the blue light GaN layer behind the well is an unintentionally doped GaN layer, and the thickness is 7nm-13.8nm.
5. The green light Micro-LED epitaxial wafer according to claim 1, characterized in that: The multi-quantum well light-emitting layer further comprises a first electron injection enhancement layer and a second electron injection enhancement layer, wherein the first electron injection enhancement layer and the second electron injection enhancement layer are sequentially stacked on the pre-well blue light multi-quantum well layer; The first electron injection enhancement layer includes a first electron injection InGaN layer and a first electron injection AlGaN layer that are periodically and alternately grown, and the second electron injection enhancement layer includes a second electron injection InGaN layer and a second electron injection GaN layer that are periodically and alternately grown.
6. The green light Micro-LED epitaxial wafer according to claim 5, characterized in that: The growth period of the first electron injection enhancement layer is 2-10, the first electron injection InGaN layer is an unintentionally doped InGaN layer, the In component accounts for 0.03-0.12, and the thickness is 0.5nm-2.5nm; the first electron injection AlGaN layer is a Si-doped AlGaN layer, the Al component accounts for 0.02-0.25, and the Si doping concentration is 1.65×10 17 cm -3 ~5.2×10 18 cm -3 , thickness is 0.8nm~3nm.
7. The green light Micro-LED epitaxial wafer according to claim 5, characterized in that: The growth period of the second electron injection enhancement layer is 2 to 5; the second electron injection InGaN layer is an unintentionally doped InGaN layer, the In component ratio is 0.01 to 0.08, and the thickness is 0.5 nm to 2.5 nm; the second electron injection GaN layer is a Si-doped GaN layer, and the Si doping concentration is 1.5×10 17 cm -3 ~3.6×10 18 cm -3 , thickness is 0.8nm~3nm.
8. A method for preparing a green light Micro-LED epitaxial wafer, used for preparing the green light Micro-LED epitaxial wafer as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: Providing a substrate, and sequentially growing a buffer layer, an N-type semiconductor layer, a low-temperature stress release layer, a multi-quantum well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer on the substrate; The multi-quantum well light-emitting layer comprises a pre-well multi-quantum well layer, a green light multi-quantum well layer and a post-well multi-quantum well layer sequentially stacked on the low-temperature stress release layer; The pre-well blue light multi-quantum well layer includes a pre-well blue light InGaN layer and a pre-well blue light GaN layer that are periodically and alternately grown, the green light multi-quantum well layer includes a green light InGaN layer and a green light GaN layer that are periodically and alternately grown, and the post-well blue light multi-quantum well layer includes a post-well blue light InGaN layer and a post-well blue light GaN layer that are periodically and alternately grown; The proportion of In in the green light InGaN layer is greater than the proportion of In in the blue light InGaN layer before the well and the blue light InGaN layer after the well; The pre-well blue light GaN layer, the green light GaN layer and the post-well blue light GaN layer all include a first GaN barrier layer, an AlGaN barrier layer and a second GaN barrier layer stacked in sequence; the Al component ratio of the AlGaN barrier layer in the pre-well blue light GaN layer, the Al component ratio of the AlGaN barrier layer in the green light GaN layer, and the Al component ratio of the AlGaN barrier layer in the post-well blue light GaN layer decrease in sequence.
9. The method for preparing a green light Micro-LED epitaxial wafer according to claim 8, characterized in that: In the pre-well blue light multi-quantum well layer, the growth temperature of the pre-well blue light InGaN layer is 750°C to 900°C, and the growth pressure is 50torr to 300torr; the growth temperature of the pre-well blue light GaN layer is 830°C to 920°C, and the growth pressure is 50torr to 300torr; In the green multi-quantum well layer, the growth temperature of the green InGaN layer is 706°C to 890°C, and the growth pressure is 50torr to 300torr; the growth temperature of the green GaN layer is 830°C to 920°C, and the growth pressure is 50torr to 300torr; In the back-well blue light multi-quantum well layer, the growth temperature of the back-well blue light InGaN layer is 750° C. to 900° C., and the growth pressure is 50 torr to 300 torr; the growth temperature of the back-well blue light GaN layer is 830° C. to 920° C., and the growth pressure is 50 torr to 300 torr; The pre-well blue light GaN layer, the green light GaN layer and the post-well blue light GaN layer all include a first GaN barrier layer, an AlGaN barrier layer and a second GaN barrier layer stacked in sequence, wherein the growth temperature of the first GaN barrier layer is 800°C~920°C, and the growth pressure is 50torr~300torr, the growth temperature of the AlGaN barrier layer is 800°C~920°C, and the growth pressure is 50torr~300torr, and the growth temperature of the second GaN barrier layer is 800°C~920°C, and the growth pressure is 50torr~300torr.
10. The method for preparing a green light Micro-LED epitaxial wafer according to claim 8, characterized in that: The invention also includes sequentially growing a first electron injection enhancement layer and a second electron injection enhancement layer on the pre-well blue light multi-quantum well layer; the first electron injection enhancement layer includes a first electron injection InGaN layer and a first electron injection AlGaN layer that are periodically and alternately grown, and the second electron injection enhancement layer includes a second electron injection InGaN layer and a second electron injection GaN layer that are periodically and alternately grown; In the first electron injection enhancement layer, the growth temperature of the first electron injection InGaN layer is 780°C to 890°C, and the growth pressure is 50torr to 300torr; the growth temperature of the first electron injection AlGaN layer is 780°C to 890°C, and the growth pressure is 50torr to 300torr; In the second electron injection enhancement layer, the growth temperature of the second electron injection InGaN layer is 780°C~890°C, and the growth pressure is 50torr~300torr; the growth temperature of the second electron injection GaN layer is 780°C~890°C, and the growth pressure is 50torr~300torr.