Lithium ferrite lithium supplement agent and preparation method thereof

By using a combination of Fe-MOFs with lithium salts and biomass graphene quantum dots in lithium-ion batteries to prepare lithium ferrite lithium supplements, the problems of irreversible loss of lithium ions and structural degradation of electrode materials in lithium-ion batteries are solved, achieving It improves the performance and environmentally friendly preparation of lithium-ion batteries and has broad application prospects.

CN118782803AActive Publication Date: 2024-10-15HUNAN SMART VALLEY NEW ENERGY TECHNOLOGY RESEARCH INSTITUTE CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411138281.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-10-15
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

Existing lithium-ion battery technology faces problems such as irreversible loss of lithium ions, structural degradation of electrode materials, complex preparation processes, and high costs, resulting in gradual degradation of battery performance and insufficient environmental protection.

Method used

Fe-MOFs is used as a synthesis template, and lithium salts, iron salts and biomass graphene quantum dots are calcined in a nitrogen atmosphere to prepare lithium ferrite lithium replenishing agent to ensure the uniform distribution and structural stability of lithium ions, using mild reaction conditions and Environmentally friendly reagents, reducing energy consumption and production costs.

Benefits of technology

Significantly improves the performance and service life of lithium-ion batteries, reduces irreversible losses, increases the actual capacity and energy density of the battery, enhances the conductivity and structural stability of electrode materials, reduces the increase in internal resistance and performance degradation, and has better sustainability and economic value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782803A_ABST
    Figure CN118782803A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to a lithium ferrite lithium supplement agent and a preparation method thereof. The lithium ferrite lithium supplement agent comprises the following components: ferric salt, an organic ligand, lithium salt, a regulator and biomass graphene quantum dots, the method comprises the following steps: firstly, synthesizing Fe-MOFs with defects as a template, mixing the Fe-MOFs with a lithium salt, an iron salt and biomass graphene quantum dots, and calcining in a nitrogen atmosphere to obtain the lithium ferrite lithium supplement agent. The Fe-MOFs are used as a synthesis template, so that lithium ions can be uniformly distributed, the local stress and volume change in the battery are reduced, meanwhile, the conductivity of the lithium supplementing agent can be improved by introducing the biomass graphene quantum dots, and the overall performance of the lithium supplementing agent can be improved through the synergistic effect of the biomass graphene quantum dots and the Fe-MOFs; and an efficient and green solution is provided for optimization of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium ferrite lithium supplement and a preparation method thereof. Background Art

[0002] Existing lithium-ion battery technology faces multiple challenges, including irreversible loss of lithium ions, structural degradation of electrode materials, and complex and costly preparation processes. During the charge and discharge process, some lithium ions are irreversibly consumed to form a solid electrolyte interface (SEI) film or participate in side reactions, causing the battery capacity to gradually decrease. These irreversibly lost lithium ions can no longer participate in subsequent electrochemical reactions, causing the battery performance to gradually decay. At the same time, the electrode material undergoes volume changes and structural degradation during repeated lithium ion insertion and deinsertion, which reduces the mechanical stability of the battery, thereby affecting its cycle life and causing an increase in internal resistance, seriously affecting the overall performance of the battery.

[0003] Lithium replenishment technology aims to restore and improve battery performance by replenishing lithium ions consumed in the battery. However, traditional lithium replenishment technology makes it difficult to ensure uniform distribution of lithium replenishers, resulting in the formation of local areas with excessively high or low lithium concentrations inside the battery. This uneven distribution will aggravate the local stress and volume changes of the battery, further affecting the cycle stability and safety of the battery. In addition, the preparation process of lithium replenishers usually requires high-temperature and long-term calcination, with complex steps and high energy consumption, which not only increases production costs, but may also introduce impurities, affecting the purity and performance consistency of the lithium replenisher. The traditional preparation process often uses organic solvents and high-temperature calcination, and the harmful gases and waste liquids produced pollute the environment, limiting the sustainability of large-scale applications. The existing technology has limited improvements in environmental protection and efficient preparation, which restricts the widespread application of lithium replenishers. Summary of the invention

[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a lithium ferrite lithium supplement and a preparation method thereof. The present invention uses defective Fe-MOFs as a synthesis template, mixes with lithium salts, iron salts and biomass graphene quantum dots, and calcines in a nitrogen atmosphere to obtain a lithium ferrite lithium supplement, which solves the problem of irreversible loss of lithium ions in existing lithium ion battery technology, while making lithium ions evenly distributed, reducing local stress and volume changes inside the battery, and using mild reaction conditions and environmentally friendly reagents to reduce energy consumption and production costs.

[0005] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: The present invention proposes a lithium ferrite lithium supplement, which includes the following components: iron salt, organic ligand, lithium salt, regulator and biomass graphene quantum dots.

[0006] Preferably, the iron salt is one or more of ferric chloride, ferric nitrate, ferric sulfate and ferric oxalate.

[0007] Preferably, the organic ligand is any one of terephthalic acid, biphenyl-4-4'-dicarboxylic acid, trimesic acid, 2-aminoterephthalic acid and 2,5-dihydroxyterephthalic acid.

[0008] Preferably, the lithium salt is one or more of lithium carbonate, lithium hydroxide, lithium nitrate, lithium sulfate, lithium sulfide, lithium oxide and lithium acetate.

[0009] Preferably, the regulator is any one of benzoic acid, formic acid and acetic acid.

[0010] Furthermore, the method for preparing biomass graphene quantum dots comprises the following steps:

[0011] ①, wash the biomass waste with clean water, dry it and put it into a grinder to grind it into biomass powder with a diameter of 2mm, then put it into an oven for carbonization at 300℃ for 40-60min to obtain carbonized biomass;

[0012] ②, weigh 4-6g of the carbonized biomass obtained in step ①, slowly add it into 100mL of concentrated sulfuric acid, slowly stir and drop 50mL of 0.5mol / L ammonium persulfate solution, slowly stir at 200-300rpm at room temperature for 2-4h, add 100mL of deionized water and mix evenly, heat to 90-95℃ and continue stirring for 10-20min, drop 100mL of 3wt% H 2 O 2 The solution was stirred for 20 min, filtered to obtain the precipitate, washed three times with deionized water, and subjected to 300 W ultrasonic stripping for 30-40 min, and filtered to obtain the biomass graphene;

[0013] ③. Disperse the biomass graphene obtained in step ② in 200-300 mL of deionized water, add 2 mL of 1 wt% ammonia water, stir at 350-450 rpm for 30 min, then transfer to a high-pressure reactor containing a polytetrafluoroethylene liner, heat at 200 ° C for 6-8 h, cool to room temperature and filter to obtain the product, wash the product three times with ethanol and deionized water alternately, and obtain biomass graphene quantum dots after drying.

[0014] Preferably, the biomass waste in step ① is any one of corn straw, wheat straw and cotton straw.

[0015] The present invention also provides a method for preparing a lithium ferrite lithium supplement, which specifically comprises the following steps:

[0016] S1. Weigh the iron salt, organic ligand and regulator, dissolve them in DMF, mix them evenly, transfer them to a reactor, heat them at 140-160°C for 12-24h, cool them to room temperature, wash them alternately with ethanol and water three times, and dry them to obtain Fe-MOFs;

[0017] S2. Add the Fe-MOFs prepared in step S1 into ethanol and disperse them evenly, then add lithium salt, iron salt and biomass graphene quantum dots, stir at 300-400 rpm for 2-4 hours, freeze-dry to obtain a reaction precursor, place it in a nitrogen atmosphere, heat it to 600-800° C. at a heating rate of 5-8° C. / min, calcine it for 1-2 hours, and cool it to room temperature to obtain a lithium supplement.

[0018] Preferably, in step S1, the usage ratio of the iron salt, the organic ligand, the regulator and DMF is 10 mmol: 10 mmol: 20-50 mmol: 20-30 mL.

[0019] Preferably, in step S2, the usage ratio of Fe-MOFs, ethanol, lithium salt, iron salt and biomass graphene quantum dots is 2-4 g: 60-100 mL: 0.1-0.2 mol: 0.1 mol: 0.2-0.5 g.

[0020] The beneficial effects achieved by the present invention are as follows:

[0021] The present invention significantly improves the performance and service life of lithium-ion batteries by using a lithium ferrite lithium supplement. The lithium ferrite lithium supplement can effectively supplement the lithium ions consumed in the battery, reduce irreversible losses, and improve the actual capacity and energy density of the battery. As a precursor material, the iron-based metal organic framework (Fe-MOFs) has a high specific surface area and a highly ordered pore structure, so that the lithium ferrite has a higher structural order and dispersibility during the formation process, provides more active sites, and significantly improves the electrochemical performance and stability of the lithium supplement. The introduction of Fe-MOFs also improves the uniform distribution of lithium ions and reduces the damage caused by local stress and volume changes inside the battery. The introduction of biomass graphene quantum dots further enhances the conductivity of the electrode material. Biomass graphene quantum dots not only have excellent conductivity themselves, but also their nanometer size and high surface area can synergize with the Fe-MOFs structure, further improving the overall performance of the lithium supplement. The synergistic effect of graphene quantum dots and Fe-MOFs ensures the structural stability of the electrode material, reduces the increase of internal resistance and performance degradation, and improves the cycle stability and safety of the battery. In general, the present invention optimizes the composition and preparation method of the lithium supplement, adopts mild reaction conditions and environmentally friendly reagents, avoids high-temperature and long-term calcination processes, reduces energy consumption and production costs, and has better sustainability and environmental friendliness. This technical solution not only solves many problems in the prior art, but also provides an efficient and green solution for the optimization of lithium-ion batteries, with broad application prospects and economic value. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 is a transmission electron microscope image of the biomass graphene quantum dots prepared in Example 1;

[0024] Figure 2 is the XRD pattern of biomass graphene quantum dots prepared in Example 1;

[0025] Figure 3 is a transmission electron microscope image of the lithium ferrite lithium supplement prepared in Example 1;

[0026] Figure 4 This is the XRD diagram of the lithium ferrite lithium supplement prepared in Example 1. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below through examples and comparative examples, but this should not be understood as the scope of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.

[0028] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples and comparative examples are purchased from commercial channels unless otherwise specified.

[0029] Example 1: This example proposes a lithium ferrite lithium supplement, which includes the following components: ferric chloride, terephthalic acid, lithium carbonate, benzoic acid and biomass graphene quantum dots.

[0030] The method for preparing biomass graphene quantum dots comprises the following steps:

[0031] ①, Wash the corn stalks with clean water, dry them and put them into a grinder to grind them into biomass powder with a diameter of 2 mm, then put them into an oven for carbonization at 300°C for 40 minutes to obtain carbonized biomass;

[0032] ②, weigh 6g of the carbonized biomass obtained in step ①, slowly add it into 100mL of concentrated sulfuric acid, slowly stir and drop 50mL of 0.5mol / L ammonium persulfate solution, slowly stir at 300rpm for 4h at room temperature, add 100mL of deionized water and mix evenly, heat to 95℃ and continue stirring for 20min, drop 100mL of 3wt% H 2 O 2 The solution was stirred for 20 min, filtered to obtain the precipitate, washed three times with deionized water, and subjected to 300 W ultrasonic stripping for 40 min, and filtered to obtain the biomass graphene;

[0033] ③. Disperse the biomass graphene obtained in step ② in 300 mL of deionized water, add 2 mL of 1 wt% ammonia water, stir at 400 rpm for 30 min, then transfer to a high-pressure reactor containing a polytetrafluoroethylene liner, heat at 200 ° C for 8 h, cool to room temperature and filter to obtain the product, wash the product three times with ethanol and deionized water alternately, and obtain biomass graphene quantum dots after drying.

[0034] This embodiment also provides a method for preparing a lithium ferrite lithium supplement, which specifically comprises the following steps:

[0035] S1. Weigh 10 mmol of ferric chloride, 10 mmol of terephthalic acid and 40 mmol of benzoic acid, dissolve them in 20 mL of DMF, mix them evenly, transfer them to a reactor and heat them at 160 °C for 12 h. After cooling to room temperature, wash them alternately with ethanol and water three times, and dry them to obtain Fe-MOFs.

[0036] S2. Weigh 4 g of the Fe-MOFs prepared in step S1 and add it to 100 mL of ethanol and disperse it evenly. Then add 0.2 mol of lithium carbonate, 0.1 mol of ferric chloride and 0.4 g of biomass graphene quantum dots. Stir at 400 rpm for 2 h in a sealed state. Freeze-dry to obtain a reaction precursor. Place it in a nitrogen atmosphere, heat it to 800 ° C at a heating rate of 5 ° C / min, calcine it for 2 h, and cool it to room temperature to obtain a lithium supplement.

[0037] Example 2: This example proposes a lithium ferrite lithium supplement, which includes the following components: ferric nitrate, trimesic acid, lithium nitrate, acetic acid and biomass graphene quantum dots.

[0038] The method for preparing biomass graphene quantum dots comprises the following steps:

[0039] ①, wash the wheat straw with clean water, dry it and put it into a grinder to grind it into biomass powder with a diameter of 2 mm, then put it into an oven for carbonization at 300°C for 60 minutes to obtain carbonized biomass;

[0040] ②, weigh 5g of the carbonized biomass obtained in step ①, slowly add it into 100mL of concentrated sulfuric acid, slowly stir and drop 50mL of 0.5mol / L ammonium persulfate solution, slowly stir at 200rpm for 2h at room temperature, add 100mL of deionized water and mix evenly, heat to 90℃ and continue stirring for 10min, drop 100mL of 3wt% H 2 O 2 The solution was stirred for 20 min, filtered to obtain the precipitate, washed three times with deionized water, and subjected to 300 W ultrasonic stripping for 30 min, and filtered to obtain the biomass graphene;

[0041] ③. Disperse the biomass graphene obtained in step ② in 200 mL of deionized water, add 2 mL of 1 wt% ammonia water, stir at 350 rpm for 30 min, then transfer to a high-pressure reactor containing a polytetrafluoroethylene liner, heat at 200 ° C for 6 h, cool to room temperature and filter to obtain the product, wash the product three times with ethanol and deionized water alternately, and obtain biomass graphene quantum dots after drying.

[0042] This embodiment also provides a method for preparing a lithium ferrite lithium supplement, which specifically comprises the following steps:

[0043] S1. Weigh 10 mmol of ferric chloride, 10 mmol of terephthalic acid and 50 mmol of benzoic acid, dissolve them in 30 mL of DMF, mix them evenly, transfer them to a reactor and heat them at 140-160 ° C for 12-24 h. After cooling to room temperature, wash them alternately with ethanol and water three times, and dry them to obtain Fe-MOFs.

[0044] S2. Weigh 2 g of the Fe-MOFs prepared in step S1 and add it to 60 mL of ethanol to disperse evenly. Then add 0.1 mol of lithium carbonate, 0.1 mol of ferric chloride and 0.2 g of biomass graphene quantum dots. Stir at 300 rpm for 4 h in a sealed state. Freeze-dry to obtain a reaction precursor. Place it in a nitrogen atmosphere, heat it to 700 ° C at a heating rate of 8 ° C / min, calcine it for 1 h, and cool it to room temperature to obtain a lithium supplement.

[0045] Example 3: This example proposes a lithium ferrite lithium supplement, which includes the following components: ferrous sulfate, biphenyl-4-4'-dicarboxylic acid, lithium acetate, formic acid and biomass graphene quantum dots.

[0046] The method for preparing biomass graphene quantum dots comprises the following steps:

[0047] ①, Wash the cotton straw with clean water, dry it and put it into a grinder to grind it into biomass powder with a diameter of 2mm, then put it into an oven for carbonization at 300℃ for 50min to obtain carbonized biomass;

[0048] ②, weigh 4g of the carbonized biomass obtained in step ①, slowly add it into 100mL of concentrated sulfuric acid, slowly stir and drop 50mL of 0.5mol / L ammonium persulfate solution, slowly stir at 260rpm for 3h at room temperature, add 100mL of deionized water and mix evenly, heat to 92℃ and continue stirring for 10-20min, drop 100mL of 3wt% H 2 O 2 The solution was stirred for 20 min, filtered to obtain the precipitate, washed three times with deionized water, and subjected to 300 W ultrasonic stripping for 35 min, and filtered to obtain the biomass graphene;

[0049] ③. Disperse the biomass graphene obtained in step ② in 250 mL of deionized water, add 2 mL of 1 wt% ammonia water, stir at 450 rpm for 30 min, then transfer to a high-pressure reactor containing a polytetrafluoroethylene liner, heat at 200 ° C for 7 h, cool to room temperature and filter to obtain the product, wash the product three times with ethanol and deionized water alternately, and obtain biomass graphene quantum dots after drying.

[0050] This embodiment also provides a method for preparing a lithium ferrite lithium supplement, which specifically comprises the following steps:

[0051] S1. Weigh 10 mmol of ferric chloride, 10 mmol of terephthalic acid and 20 mmol of benzoic acid, dissolve them in 25 mL of DMF, mix them evenly, transfer them to a reactor and heat them at 150 °C for 16 h. After cooling to room temperature, wash them alternately with ethanol and water three times, and dry them to obtain Fe-MOFs.

[0052] S2. Weigh 3 g of the Fe-MOFs prepared in step S1 and add it to 80 mL of ethanol and disperse it evenly. Then add 0.15 mol of lithium salt, 0.1 mol of iron salt and 0.5 g of biomass graphene quantum dots. Stir at 360 rpm for 3 h in a closed state. Freeze-dry to obtain a reaction precursor. Place it in a nitrogen atmosphere, heat it to 600 ° C at a heating rate of 7 ° C / min, calcine it for 1.5 h, and cool it to room temperature to obtain a lithium supplement.

[0053] Comparative Example 1: This comparative example proposes a lithium ferrite lithium supplement agent, which differs from Example 1 in that Fe-MOFs is not used, and the remaining components, component contents, and experimental steps are the same as those in Example 1. The lithium ferrite lithium supplement agent includes the following components: ferric chloride, lithium carbonate, and biomass graphene quantum dots.

[0054] The method for preparing biomass graphene quantum dots comprises the following steps:

[0055] ①, Wash the corn stalks with clean water, dry them and put them into a grinder to grind them into biomass powder with a diameter of 2 mm, then put them into an oven for carbonization at 300°C for 40 minutes to obtain carbonized biomass;

[0056] ②, weigh 6g of the carbonized biomass obtained in step ①, slowly add it into 100mL of concentrated sulfuric acid, slowly stir and drop 50mL of 0.5mol / L ammonium persulfate solution, slowly stir at 300rpm for 4h at room temperature, add 100mL of deionized water and mix evenly, heat to 95℃ and continue stirring for 20min, drop 100mL of 3wt% H 2 O 2 The solution was stirred for 20 min, filtered to obtain the precipitate, washed three times with deionized water, and subjected to 300 W ultrasonic stripping for 40 min, and filtered to obtain the biomass graphene;

[0057] ③. Disperse the biomass graphene obtained in step ② in 300 mL of deionized water, add 2 mL of 1 wt% ammonia water, stir at 400 rpm for 30 min, then transfer to a high-pressure reactor containing a polytetrafluoroethylene liner, heat at 200 ° C for 8 h, cool to room temperature and filter to obtain the product, wash the product three times with ethanol and deionized water alternately, and obtain biomass graphene quantum dots after drying.

[0058] This comparative example also proposes a method for preparing a lithium ferrite lithium supplement, which specifically comprises the following steps:

[0059] S1. Add 0.2 mol lithium carbonate, 0.1 mol ferric chloride and 0.4 g biomass graphene quantum dots into 100 mL ethanol, stir at 400 rpm for 2 h, freeze-dry to obtain a reaction precursor, place it in a nitrogen atmosphere, heat it to 800 ° C at a heating rate of 5 ° C / min, calcine it for 2 h, and cool it to room temperature to obtain a lithium supplement.

[0060] Comparative Example 2: This comparative example proposes a lithium ferrite lithium supplement, which differs from Example 1 only in that biomass graphene quantum dots are not added, and the remaining components, component contents, and experimental steps are the same as those in Example 1.

[0061] Experimental Example 1: The microscopic morphology of the biomass graphene quantum dots prepared in Example 1 was observed using a transmission electron microscope; and the structural characteristics of the biomass graphene quantum dots prepared in Example 1 were analyzed using X-ray diffraction.

[0062] Figure 1 This is a transmission electron microscope image of the biomass graphene quantum dots prepared in Example 1. As shown in the figure, the biomass graphene quantum dots have a small particle size and are evenly distributed, with a diameter of about 4 nm. Figure 2 This is the XRD diagram of the biomass graphene quantum dots prepared in Example 1. As shown in the figure, the diffraction peak at 25.4° corresponds to the (002) diffraction plane of the graphene quantum dots. The above analysis shows that the biomass graphene quantum dots were successfully prepared.

[0063] Experimental Example 2: The microscopic morphology of the lithium ferrite lithium supplement prepared in Example 1 was observed using a transmission electron microscope; and the structural characteristics of the lithium ferrite lithium supplement prepared in Example 1 were analyzed using X-ray diffraction.

[0064] Figure 3 This is a transmission electron microscope image of the lithium ferrite supplement prepared in Example 1. As shown in the figure, the MOFs structure collapses, but the overall shape is still a cubic nanoparticle, and the particle size is small, with a diameter of about 120nm. Figure 4 This is the XRD diagram of the lithium ferrite lithium supplement prepared in Example 1. As shown in the figure, the diffraction peaks in the figure correspond to the reflections of the (221), (220), (311), (317), (400), (417), (419), (422), (440) and (511) planes of lithium ferrite, respectively. At the same time, the reflection of the (002) diffraction plane of the graphene quantum dots can be observed, indicating that the lithium ferrite lithium supplement was successfully prepared.

[0065] Experimental Example 3: Performance Test:

[0066] (1) Half-cell performance test: The lithium ferrite supplement prepared in Examples 1-3 and Comparative Examples 1-2 was mixed with conductive carbon black, PVDF, and NMP in a mass ratio of 90:5:5:60 to form a positive electrode slurry, which was evenly coated on an aluminum foil substrate, vacuum dried at 80°C for 12 hours, rolled and cut to obtain a positive electrode sheet, and a lithium sheet was used as the negative electrode. In a CR2032 button battery shell, the positive electrode sheet, lithium sheet, and polyethylene film (diaphragm) were assembled together, 1 mol / L LiPF6 / EC+DMC+EMC electrolyte was added, and sealed. In a 25°C constant temperature box, charge to 4.5V at a current of 0.1C, and then discharge to 2.0V at the same current, and record the first charge specific capacity and the first charge and discharge efficiency. The test data are shown in Table 1.

[0067] Table 1 Half-cell performance test data

[0068]

[0069]

[0070] As shown in Table 1, in the half-cell test, the first charge specific capacity of Examples 1-3 is significantly higher than that of Comparative Examples 1 and 2. This shows that the lithium ferrite lithium supplement synthesized in the examples can store more charge during the first charge process. At the same time, the first charge and discharge efficiency of Examples 1-3 is significantly lower than that of Comparative Examples 1 and 2, indicating that the lithium supplement prepared in Examples 1-3 effectively supplements the lithium ion loss caused by side reactions during the first charge process. Although this will reduce the first discharge efficiency, it plays a positive role in compensating for the initial irreversible lithium loss.

[0071] (2) Full battery performance test: The lithium ferrite lithium supplement prepared in Examples 1-3 and Comparative Examples 1-2 were respectively mixed with lithium iron phosphate, conductive carbon black, PVDF, and N-methylpyrrolidone in a mass ratio of 10:90:5:5:60 to form a positive electrode slurry, which was evenly coated on an aluminum foil substrate, vacuum dried at 80°C for 12 hours, rolled, and cut to obtain a positive electrode sheet. Graphite, conductive carbon black, CMC, SBR, and deionized water were mixed in a mass ratio of 94:2:2:2:100 to form a negative electrode slurry, which was evenly coated on a copper foil substrate, vacuum dried at 80°C for 12 hours, rolled, and cut to obtain a negative electrode sheet. The obtained positive electrode sheet, negative electrode sheet, and polyethylene film were wound into the pole core of a lithium-ion battery, and 1 mol / L LiPF 6 / EC+DMC+EMC electrolyte was injected into the battery aluminum shell and sealed to prepare a 1Ah lithium-ion battery.

[0072] Test conditions: Charge to 4.5V at 1C constant current in a 25℃ constant temperature box, then discharge to 2.0V at 1C constant current, test the initial charge and discharge capacity and the capacity retention rate after 200 cycles (1C), and calculate the unit lithium replenishment capacity. The test data are shown in Table 2.

[0073] Table 2 Full battery performance test data

[0074]

[0075] According to experimental data, the lithium ferrite lithium supplement of Examples 1-3 performs well in terms of first charge specific capacity, first discharge specific capacity, and 200 cycle capacity retention rate. Among them, the first charge specific capacity and discharge specific capacity of the embodiment are significantly higher than those of the comparative example, indicating that it has a higher initial capacity; the 200 cycle capacity retention rate is between 97.47% and 98.13%, showing excellent cycle stability. In contrast, the cycle capacity retention rate of the comparative example is significantly lower, which verifies the significant advantages of the lithium ferrite lithium supplement of the embodiment of the present invention in improving battery performance and extending service life, and has good application prospects.

[0076] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A lithium ferrite lithium supplement, characterized in that: The lithium ferrite lithium supplement comprises the following components: iron salt, organic ligand, lithium salt, regulator and biomass graphene quantum dots; The method for preparing biomass graphene quantum dots comprises the following steps: ①, wash the biomass waste, dry and crush it into biomass powder, and then carbonize it at 300℃ for 40-60min to obtain carbonized biomass; ②, the carbonized biomass obtained in step ①, slowly add concentrated sulfuric acid, slowly stir and drop ammonium persulfate solution, slowly stir at room temperature for 2-4h, add deionized water and mix evenly, heat to 90-95°C and continue stirring for 10-20min, drop H2O2 solution, continue stirring for 20min, filter to obtain precipitate, wash and ultrasonically peel for 30-40min, filter to obtain biomass graphene; ③. Disperse the biomass graphene obtained in step ② in deionized water, add ammonia water and stir for 30 minutes, then transfer to a high-pressure reactor, heat at 200° C. for 6 to 8 hours, cool to room temperature and filter to obtain the product, and then wash and dry to obtain biomass graphene quantum dots.

2. The lithium ferrite supplement according to claim 1, characterized in that: The iron salt is one or more of ferric chloride, ferric nitrate, ferric sulfate and ferric oxalate.

3. The lithium ferrite supplement according to claim 2, characterized in that: The organic ligand is any one of terephthalic acid, biphenyl-4-4'-dicarboxylic acid, trimesic acid, 2-aminoterephthalic acid and 2,5-dihydroxyterephthalic acid.

4. The lithium ferrite supplement according to claim 3, characterized in that: The lithium salt is one or more of lithium carbonate, lithium hydroxide, lithium nitrate, lithium sulfate, lithium sulfide, lithium oxide and lithium acetate.

5. The lithium ferrite supplement according to claim 4, characterized in that: The regulator is any one of benzoic acid, formic acid and acetic acid.

6. The lithium ferrite supplement according to claim 5, characterized in that: Preferably, the biomass waste in step ① is any one of corn straw, wheat straw and cotton straw.

7. A method for preparing the lithium ferrite lithium supplement according to any one of claims 1 to 6, characterized in that: The specific steps include: S1. Weigh the iron salt, organic ligand and regulator, dissolve them in DMF, mix them evenly, transfer them to a reactor, heat them at 140-160°C for 12-24h, cool them to room temperature, wash them alternately with ethanol and water three times, and dry them to obtain Fe-MOFs; S2. Add the Fe-MOFs prepared in step S1 into ethanol and disperse them evenly, then add lithium salt, iron salt and biomass graphene quantum dots, stir in a closed state for 2 to 4 hours, freeze-dry to obtain a reaction precursor, place it in a nitrogen atmosphere, heat it to 600 to 800° C. at a heating rate of 5 to 8° C. / min, calcine it for 1 to 2 hours, and cool it to room temperature to obtain a lithium supplement.

Citation Information

Patent Citations

  • Positive electrode lithium supplement additive and preparation method and application thereof

    CN114709421A

  • Preparation method of negative electrode lithium supplement additive

    CN117352676A

  • Lithium-rich composite material and preparation method and application thereof

    CN118136802A

  • Positive lithium supplementing material, preparation method thereof, positive plate and battery

    CN118299691A

  • Composite lithium supplement agent as well as preparation method and application thereof

    CN118507701A