Preparation method of fuel cell oxygen reduction catalyst

Through vacuum heating and molecular cross-linking agent self-assembly technology, Pt or PtM alloy nanoparticles are grown in situ in the carbon pores of the fuel cell catalyst, which solves the problems of agglomeration and corrosion of the catalyst in acidic media and high potential, and significantly improves the performance of the catalyst. durability and stability.

CN118782816APending Publication Date: 2024-10-15KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410906786.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing fuel cell oxygen reduction catalysts are prone to agglomeration, corrosion and shedding of Pt-based alloy nanoparticles in acidic media and high potentials, resulting in reduced catalyst activity and attenuation of fuel cell performance.

Method used

Vacuum heating of porous carbon materials is used, combined with the self-assembly of molecular cross-linking agents in carbon channels and the chemical coordination adsorption of Pt or PtM precursors, to achieve the preparation of in-situ growth of Pt or PtM alloy nanoparticles in carbon channels to enhance the performance of the catalyst. Interaction and stability.

Benefits of technology

It significantly improves the durability and stability of the Pt-based catalyst for the fuel cell cathode, prevents the agglomeration, corrosion and shedding of the catalyst at low and high potentials, and extends the service life of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782816A_ABST
    Figure CN118782816A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a fuel cell oxygen reduction catalyst, and belongs to the technical field of fuel cell catalysts. The preparation method comprises the following steps: firstly, heating and exhausting a porous carbon material under high vacuum, then carrying out ultrasonic treatment under a vacuum environment and a normal-temperature and normal-pressure environment, and generating pi-pi interaction between a molecular crosslinking agent in a molecular crosslinking agent mixed solution and porous carbon, so that crosslinking agent molecules are self-assembled in carbon pore channels with different sizes according to the sizes of the crosslinking agent molecules. Secondly, metal ions in the metal precursor solution are coordinated with chemical groups assembled on benzene rings in the molecular cross-linking agent in the carbon pore channels through ultrasound, and then the metal ions are chemically adsorbed into the pore channels of the porous carbon material. And finally, reducing the metal ions in the pore channels of the carbon material through an in-situ reduction reaction, and carrying out in-situ nucleation and growth to form a nanostructure of carbon pore confinement Pt or PtM alloy nanoparticles. The catalyst is used as a cathode oxygen reduction catalyst of a proton exchange membrane fuel cell, has relatively high oxygen reduction activity and stability under an acidic condition, and particularly has good durability under a high potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cell catalysts, and in particular relates to a method for preparing a fuel cell oxygen reduction catalyst. Background Art

[0002] Fuel cells are the most promising green energy batteries to replace traditional internal combustion engines in the future. Fuel cells are mainly composed of electrocatalysts, proton exchange membranes, bipolar plates and carbon paper. Numerous studies have shown that the key material for fuel cells to achieve energy conversion is the electrocatalyst. Among them, the reaction rate of cathode oxygen reduction reaction (ORR) is much slower than that of anode hydrogen oxidation (HOR). Excellent Pt-based catalysts are needed to overcome the problem of slow ORR kinetics. At present, fuel cell oxygen reduction catalysts are mainly carbon-supported Pt nanoparticle catalysts (Pt / C) or carbon-supported Pt-based alloy nanoparticle catalysts (PtM / C) formed by alloying Pt with transition metals (M=Ni, Co, Cu and Fe, etc.). Regulating the size, morphology and structure of metal nanoparticles can make Pt / C or PtM / C catalysts obtain high catalytic activity. However, under the actual operating conditions of fuel cells, factors such as agglomeration of Pt-based alloy nanoparticles, leaching of transition metals and corrosion of carbon carriers caused by high potential cycles will shorten the catalyst life and thus affect the performance of fuel cells. For example, when the cathode oxygen reduction catalyst of the fuel cell is in an acidic medium (pH < 1), with high oxygen concentration and the electrode potential at a dynamic potential of 0.6 to 1.5 V, the agglomeration and migration of Pt-based alloy nanoparticles, the loss of alloying transition metal elements and the corrosion of the carbon carrier will directly lead to the overall performance degradation of the fuel cell. These problems have become the difficult problems that need to be broken through in basic research and practical application. Therefore, improving the interaction between nanoparticles and carbon carriers and enhancing the corrosion resistance of carbon carriers, and then developing the preparation technology of high-performance Pt / C or PtM / C catalysts are of great significance for the commercial application of fuel cells.

[0003] At present, the carbon carriers of fuel cell cathode oxygen reduction catalysts mainly use solid carbon and porous carbon. Solid carbon has a medium surface area and a high degree of graphitization, so it has good resistance to carbon corrosion. However, in Pt / C or PtM / C catalysts prepared from solid carbon, metal nanoparticles are mainly dispersed on the surface of solid carbon. During the preparation of membrane electrode, sulfur-containing ionomers will poison Pt, and metal nanoparticles are prone to agglomeration during the electrochemical reaction, resulting in reduced catalyst activity. Porous carbon has a high surface area (500-2000m 2 / g) and has a large number of pores and channels inside. There are mainly three types of pores inside, which can be divided into micropores (<2nm), mesopores (2-50nm) and macropores (>50nm) according to the pore size. In particular, the tiny channels in porous carbon have very small openings (1-4nm), and the channels themselves are tortuous, making it difficult for metal precursor solutions to enter them, which makes it difficult for metal ions to grow in situ in these channels. At present, most patents and literature reports that the preparation method of Pt / C or PtM / C catalyst is mainly: first, a certain amount of porous carbon is placed in a Pt salt precursor solution or a PtM mixed precursor solution of a Pt salt and a transition metal salt, stirred and ultrasonically treated, and then reduced to metal atoms by a low-temperature and high-pressure liquid phase or high-temperature solid phase reduction method, and the metal atoms are nucleated and grown to form Pt or PtM alloy nanoparticles. Although the obtained Pt / C or PtM / C catalyst has high activity, the stability of the catalyst is not good during the electrochemical process. This is mainly because the Pt or PtM alloy nanoparticles in the Pt-based catalyst are dispersed on the surface of the porous carbon, but not dispersed in the porous carbon pores. This causes the Pt or PtM alloy nanoparticles in the Pt-based catalyst to fall off easily and agglomerate during the operation of the fuel cell at a low potential (<1.0V), resulting in the degradation of the fuel cell performance. On the other hand, the frequent starting / braking voltage of fuel cell vehicles during long-term operation will reach about 1.5V, which will cause corrosion of the carbon carrier and also cause degradation of the fuel cell performance. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides a method for preparing a fuel cell oxygen reduction catalyst.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a fuel cell oxygen reduction catalyst, comprising the following steps:

[0006] (1) placing the porous carbon material in a vacuum environment, heating and keeping the temperature to remove residual gas, and then cooling;

[0007] (2) adding a molecular crosslinking agent to an organic solvent, stirring and ultrasonicating to obtain a crosslinking agent mixed solution, then dropping the crosslinking agent mixed solution onto the porous carbon material under a vacuum environment, and after the crosslinking agent mixed solution completely submerges the porous carbon material, ultrasonicating under vacuum negative pressure and ultrasonicating under normal temperature and pressure in sequence to obtain a porous carbon-molecular crosslinking agent-organic solvent mixed solution;

[0008] (3) Adding a Pt salt solution or a PtM precursor solution composed of a Pt salt and a transition metal salt into a mixed solution of porous carbon-molecular crosslinking agent-organic solvent, mixing and ultrasonicating, and then hydrothermally reacting or hydrogen reduction heat treatment, and finally washing, separating, and vacuum drying to obtain a Pt / C catalyst or a PtM / C catalyst.

[0009] As a preferred embodiment of the present invention, in the steps (1) and (2), the vacuum degree of the vacuum environment is 100 Pa to 10 -3 Pa; in the step (1), the heating temperature is 50 to 350°C and the insulation time is 0.5 to 5h.

[0010] As a preferred embodiment of the present invention, the molecular cross-linking agent is at least one of phenol, benzoic acid, phenylacetic acid, methyl benzoate, ethyl benzoate, naphthoic acid, naphthylacetic acid, methyl naphthoate, ethyl naphthoate, anthracenecarboxylic acid, anthraceneacetic acid, methyl anthracenecarboxylate, and ethyl anthracenecarboxylate.

[0011] As a preferred embodiment of the present invention, the organic solvent is one of ethanol, ethylene glycol, methanol, benzyl alcohol, chloroform, oleic acid, oleylamine, and N,N-dimethylformamide.

[0012] As a preferred embodiment of the present invention, in the step (2), the concentration of the molecular cross-linking agent in the organic solvent is 0.1 to 10 g / L.

[0013] As a preferred embodiment of the present invention, in the step (2), ultrasound is performed for 10 to 30 seconds every 1 to 2 minutes under vacuum negative pressure, for a total of 3 to 120 minutes; ultrasound is performed for 0.5 to 10 hours at normal temperature and pressure.

[0014] As a preferred embodiment of the present invention, in step (3), the concentration of the Pt salt solution is 2 to 20 g / L; the concentration of the metal ions in the PtM precursor mixed solution is 0.5 to 30 g / L.

[0015] As a preferred embodiment of the present invention, the mass volume ratio of the porous carbon material to the PtM precursor mixed solution is 0.2-100 g / L: 0.2-100 g / L; the mass volume ratio of the porous carbon material to the Pt salt solution is 0.1-50 g / L: 0.1-50 g / L.

[0016] As a preferred embodiment of the present invention, the porous carbon material is one of Ketjen Black EC-300J, Ketjen Black EC-600JD, acetylene black, and Cabot BP2000.

[0017] As a preferred embodiment of the present invention, the temperature rise specific surface area of ​​the porous carbon material is 500 to 2000 m 2 / g, and has three types of pores and channels inside: micropores (<2nm), mesopores (2-50nm) and macropores (>50nm).

[0018] As a preferred embodiment of the present invention, in the step (2), the cross-linking agent mixed solution is added dropwise at a speed of 4 ml / min to 50 ml / min under a vacuum environment.

[0019] As a preferred embodiment of the present invention, the Pt salt is one of platinum acetate, platinum acetylacetonate, chloroplatinic acid, and platinum dichloride; the transition metal salt is one of nickel chloride hexahydrate, nickel acetylacetonate, nickel acetate, cupric chloride dihydrate, copper acetylacetonate, cupric acetate, cobalt chloride hexahydrate, cobalt acetylacetonate, cobalt acetate, ferric chloride hexahydrate, ferric acetylacetonate, and ferric acetate.

[0020] As a preferred embodiment of the present invention, in the step (4), the temperature of the hydrothermal reaction is 150-200° C. and the time is 5-60 hours.

[0021] As a preferred embodiment of the present invention, the temperature of the hydrogen reduction heat treatment is 400-900°C, the time is 1-5h, the gas is a mixture of nitrogen and hydrogen or a mixture of argon and hydrogen, the volume ratio of nitrogen to hydrogen in the mixture of nitrogen and hydrogen is 2-10:1, the volume ratio of argon to hydrogen in the mixture of argon and hydrogen is 2-10:1, and the flow rate of the mixed gas is 10-1000mL / min.

[0022] Principle of the invention: The present invention adopts the combined strategy of "vacuum heating and exhaust of porous carbon materials + self-assembly of molecular cross-linking agents in carbon pores under vacuum + chemical coordination adsorption of Pt precursor or PtM precursor molecules and molecular cross-linking agents + in-situ growth of Pt or PtM alloy nanoparticles in carbon pores" to prepare high-performance fuel cell oxygen reduction catalysts.

[0023] The present invention firstly heats the porous carbon material under the negative pressure generated by vacuum, so that the organic volatiles adsorbed inside and outside the carbon material pores by physical or chemical means and the residual gas adsorbed inside the tortuous micro-pores (1 to 4 nm) inside the carbon material are discharged and pumped away, thereby fully exposing the fresh surface inside and outside the carbon material pores, and providing a large number of clean adsorption sites for the in-situ growth of metal nanoparticles in the pores during the catalyst synthesis process. Then, ultrasound is applied under vacuum environment and normal temperature and pressure environment, and the molecular crosslinker in the molecular crosslinker mixed solution interacts with the porous carbon to self-assemble the crosslinker molecules in carbon pores of different sizes according to their own size. Secondly, ultrasound is used to coordinate the metal ions in the metal precursor solution with the chemical groups on the benzene rings in the molecular crosslinker assembled in the carbon pores, thereby chemically adsorbing the metal ions into the pores of the porous carbon material. Finally, through the in-situ reduction reaction, the metal ions are reduced in the carbon material pores and nucleated and grown in-situ to form a nanostructure of carbon pore-confined Pt or PtM alloy nanoparticles.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention obtains the nanostructure of carbon pore-confined Pt or PtM alloy nanoparticles by heating the carbon material in a vacuum, self-assembly of the crosslinker molecules on the carbon, and chemical coordination adsorption of the crosslinker molecules and Pt or transition metal M ions. First, due to the carbon pore-confined metal nanoparticles, the interaction between the porous carbon material and the metal nanoparticles is enhanced, so that the synthesized Pt-based catalyst operates for a long time in the normal working potential range (0.6-0.95V) of the fuel cell, and the agglomeration, dissolution and shedding of the Pt-based alloy nanoparticles in the catalyst are prevented, which significantly improves the durability of the Pt-based catalyst of the fuel cell cathode. Secondly, the in-situ growth of Pt and PtM alloy nanoparticles in the pores of the carbon material of the present invention can promote the interaction between the metal nanoparticles and the carbon carrier, so that the high potential corrosion of the carbon carrier at 1.0-1.50V under the frequent start-stop of the fuel cell vehicle is slowed down, and the collapse of the pore structure of the carbon material is prevented, thereby preventing the agglomeration, dissolution and shedding of the Pt-based alloy nanoparticles in the catalyst, and significantly improving the stability of the Pt-based catalyst of the fuel cell cathode. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a technical flow diagram of the method for preparing the fuel cell oxygen reduction catalyst according to the present invention.

[0027] Figure 2 TEM images of the fuel cell oxygen reduction catalyst prepared in Example 1, wherein (a) is a low-magnification TEM image and (b) is a high-magnification TEM image.

[0028] Figure 3 TEM images of the fuel cell oxygen reduction catalyst prepared in Example 2, wherein (a) is a high-magnification TEM image and (b) is a low-magnification TEM image.

[0029] Figure 4 TEM images of the fuel cell oxygen reduction catalyst prepared in Example 3, wherein (a) is a high-magnification TEM image and (b) is a low-magnification TEM image.

[0030] Figure 5 HRTEM images of the fuel cell oxygen reduction catalysts prepared in Example 2 and Comparative Example 2, where (a) is Example 2 and (b) is Comparative Example 2.

[0031] Figure 6 The X-ray diffraction patterns of the fuel cell oxygen reduction catalysts prepared in Examples 1 and 2.

[0032] Figure 7The initial CV, initial LSV, CV graph and LSV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Example 1 and Comparative Example 1, wherein (a) is the initial CV and CV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Example 1 measured in a 0.1M HClO4 solution saturated with N2; (b) is the initial CV and LSV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Example 1 measured in a 0.1M HClO4 solution saturated with O2; (c) is the initial CV and CV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Comparative Example 1 measured in a 0.1M HClO4 solution saturated with N2; (d) is the initial LSV and LSV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Comparative Example 1 measured in a 0.1M HClO4 solution saturated with O2.

[0033] Figure 8 The initial CV, initial LSV, CV graph and LSV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Example 2 and Comparative Example 2, wherein (a) is the initial CV and CV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Example 2 measured in a 0.1M HClO4 solution saturated with N2; (b) is the initial CV and LSV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Example 2 measured in a 0.1M HClO4 solution saturated with O2; (c) is the initial CV and CV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Comparative Example 2 measured in a 0.1M HClO4 solution saturated with N2; (d) is the initial LSV and LSV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Comparative Example 2 measured in a 0.1M HClO4 solution saturated with O2.

[0034] Fig. 9The initial CV, initial LSV, CV graph and LSV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Example 3 and Comparative Example 3, wherein (a) is the initial CV and CV graph after 5000 cycles at high potential measured in a 0.1M HClO4 solution saturated with N2 of the fuel cell oxygen reduction catalyst prepared in Example 3; (b) is the initial CV and LSV graph after 5000 cycles at high potential measured in a 0.1M HClO4 solution saturated with O2 of the fuel cell oxygen reduction catalyst prepared in Example 3; (c) is the initial CV and CV graph after 5000 cycles at high potential measured in a 0.1M HClO4 solution saturated with N2 of the fuel cell oxygen reduction catalyst prepared in Comparative Example 3; (d) is the initial LSV and LSV graph after 5000 cycles at high potential measured in a 0.1M HClO4 solution saturated with O2 of the fuel cell oxygen reduction catalyst prepared in Comparative Example 3.

[0035] Fig.10 The initial CV, initial LSV, CV graph and LSV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Example 4 and Comparative Example 4, wherein (a) is the initial CV and CV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Example 4 measured in a 0.1M HClO4 solution saturated with N2; (b) is the initial CV and LSV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Example 4 measured in a 0.1M HClO4 solution saturated with O2; (c) is the initial CV and CV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Comparative Example 4 measured in a 0.1M HClO4 solution saturated with N2; (d) is the initial LSV and LSV graph after 5000 cycles at high potential of the fuel cell oxygen reduction catalyst prepared in Comparative Example 4 measured in a 0.1M HClO4 solution saturated with O2.

[0036] Fig.11 The figure is a bar graph of the ORR activity (MA) loss rate of the catalysts prepared in Examples 1-4 and Comparative Examples 1-4 after 5000 cycles at high potential or 30000 cycles at low potential; (a) is a bar graph of the ORR activity (MA) loss rate of the catalysts prepared in Examples 1-4 and Comparative Examples 1-4 after 5000 cycles at high potential; (b) is a bar graph of the ORR activity (MA) loss rate of the catalysts prepared in Examples 1-4 and Comparative Examples 1-4 after 30000 cycles at low potential. DETAILED DESCRIPTION

[0037] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0038] Example 1

[0039] (1) A quartz bottle containing 1000 mg of Ketjen Black EC-300J was placed in a vacuum device with heating and ultrasound, evacuated to a vacuum degree of 100 Pa using a mechanical pump and a molecular pump, and heated to 320°C and kept warm for 3 h.

[0040] (2) A mixed solution of 500 mg of phenol and 600 ml of ethylene glycol was then injected into a quartz bottle containing 1000 mg of Ketjen Black EC-300J in a vacuum chamber at a rate of 45 ml / min using a peristaltic pump. The mixed solution of phenol, ethylene glycol and Ketjen Black EC-300J was then sonicated using an ultrasonic rod under a vacuum environment for 30 seconds every 1 minute for a total of 3 minutes to completely wet the pores of the Ketjen Black EC-300J with the mixed solution. The vacuum was then removed from the quartz bottle containing the mixed solution and sonicated for 30 minutes at room temperature and pressure.

[0041] (3) Then, 1200 mg of chloroplatinic acid and 700 mg of cobalt chloride hexahydrate were added to the mixed solution, and then ultrasonic treatment was performed for 3 hours. Finally, the mixed solution was added to an autoclave, reacted at a temperature of 150° C. for 12 hours, and cooled to room temperature. The reaction product was centrifuged, acid-washed, and then vacuum-dried to prepare a Pt3Co / C catalyst.

[0042] Example 2

[0043] A method for preparing a fuel cell oxygen reduction catalyst comprises the following steps:

[0044] (1) Place a quartz bottle containing a certain amount of Cabot BP2000 in a vacuum device with heating and ultrasound, and evacuate the vacuum to 10 -2 Pa vacuum, heated to 190℃ and kept warm for 4h.

[0045] (2) A mixed solution of 800 mg of methyl benzoate as a molecular cross-linking agent and 1000 ml of benzyl alcohol as a solvent was then injected into a quartz bottle containing 500 mg of Cabot BP2000 in a vacuum chamber at a rate of 50 ml / min using a peristaltic pump. The mixed solution of methyl benzoate, benzyl alcohol and Cabot BP2000 was then sonicated using an ultrasonic rod under vacuum conditions for 15 seconds every 1.5 minutes for a total of 5 minutes to completely wet the pores of the Cabot BP2000 with the mixed solution. The vacuum was then removed from the quartz bottle containing the mixed solution and sonicated for 3 hours at room temperature and pressure.

[0046] (3) Then, 100 mg of platinum acetylacetonate and 420 mg of cobalt acetate were added to the mixed solution, followed by ultrasonic treatment for 2 hours. Finally, the mixed solution was added to an autoclave and reacted at 160° C. for 24 hours. The mixture was cooled to room temperature, and the reaction product was centrifuged, acid-washed, and then vacuum-dried to prepare a Pt3Co / C catalyst.

[0047] Example 3

[0048] A method for preparing a fuel cell oxygen reduction catalyst comprises the following steps:

[0049] (1) Place a quartz bottle containing a certain amount of Ketjen Black EC-600JD in a vacuum device with heating and ultrasound, and evacuate the vacuum to 10 -1 Pa vacuum, heated to 150℃ and kept warm for 5h.

[0050] (2) A mixed solution of 50 mg of naphthoic acid as a molecular cross-linking agent and 30 ml of ethanol as a solvent was then injected into a quartz bottle containing 26 mg of acetylene black in a vacuum chamber at a rate of 4 ml / min using a peristaltic pump. The mixed solution of naphthoic acid, ethanol and Ketjen Black EC-600J was then ultrasonically treated with an ultrasonic rod under vacuum conditions for 20 seconds every 2 minutes for a total of 6 minutes to completely wet the pores of the Ketjen Black EC-600JD. The vacuum was then removed from the quartz bottle containing the mixed solution and ultrasonicated for 6 hours at room temperature and pressure.

[0051] (3) Then, 24 mg of platinum acetate and 5 mg of nickel acetate were added to the mixed solution, followed by ultrasonic treatment for 2.5 hours. Finally, the mixed solution was added to an autoclave and reacted at 170° C. for 36 hours. The mixture was cooled to room temperature, and the reaction product was centrifuged, acid-washed, and then vacuum-dried to prepare a Pt3Ni / C catalyst.

[0052] Example 4

[0053] A method for preparing a fuel cell oxygen reduction catalyst comprises the following steps:

[0054] (1) A quartz bottle containing a certain amount of acetylene black is placed in a vacuum device with heating and ultrasound, and evacuated to a vacuum degree of 10 Pa using a mechanical pump and a molecular pump, and then kept at 200°C for 4 hours.

[0055] (2) A mixed solution of 500 mg of anthracenecarboxylic acid as a molecular crosslinking agent and 2000 ml of N,N-dimethylformamide as a solvent was then injected into a quartz bottle containing 1000 mg of acetylene black in a vacuum chamber at a rate of 20 ml / min using a peristaltic pump. The mixed solution of anthracenecarboxylic acid, N,N-dimethylformamide and acetylene black was then ultrasonically treated with an ultrasonic rod under vacuum conditions for 25 seconds every 1.5 minutes for a total of 2 minutes to completely wet the pores of the acetylene black with the mixed solution. The vacuum was then removed from the quartz bottle containing the mixed solution and ultrasonicated for 10 hours at room temperature and pressure.

[0056] (3) Then, 3600 mg of platinum acetylacetonate and 2900 mg of copper acetate were added to the mixed solution, followed by ultrasonic treatment for 4 hours. Finally, the mixed solution was added to an autoclave and reacted at 160° C. for 48 hours. The mixture was cooled to room temperature, and the reaction product was centrifuged, acid-washed, and then vacuum-dried to prepare a PtCu / C catalyst.

[0057] Comparative Example 1

[0058] In this comparative example, no vacuum heating or molecular cross-linking agent was used in the preparation process of the catalyst, and the other experimental steps were the same as those in Example 1:

[0059] 1000 mg of Ketjen Black EC-300J was slowly added to a mixed solution of 1200 mg of chloroplatinic acid, 700 mg of cobalt chloride hexahydrate and 600 ml of ethylene glycol, and then ultrasonically treated at normal pressure for 3 hours. The mixed solution was added to an autoclave and reacted at a temperature of 150°C for 12 hours. The mixture was cooled to room temperature, and the reaction product was centrifuged, washed, acid-washed and vacuum-dried to prepare a Pt3Co / C catalyst.

[0060] Comparative Example 2

[0061] In this comparative example, no vacuum heating or molecular cross-linking agent was used in the preparation process of the catalyst, and the other experimental steps were the same as those in Example 2:

[0062] 500 mg of Cabot BP2000 was slowly added to a mixed solution of 100 mg of platinum acetylacetonate, 420 mg of cobalt acetate, and 1000 ml of benzyl alcohol, and then ultrasonically treated for 2 hours; finally, the mixed solution was added to an autoclave, reacted at a temperature of 160° C. for 24 hours, cooled to room temperature, and the reaction product was centrifuged, acid-washed, and then vacuum-dried to prepare a Pt3Co / C catalyst.

[0063] Comparative Example 3

[0064] In this comparative example, no vacuum heating or molecular cross-linking agent was used in the preparation process of the catalyst, and the other experimental steps were the same as those in Example 3:

[0065] 26 mg of Ketjen Black EC-600JD was slowly added to a mixed solution of 24 mg of platinum acetate, 5 mg of nickel acetate and 30 ml of ethanol, and ultrasonically treated for 2.5 hours at normal pressure; finally, the mixed solution was added to an autoclave, reacted at a temperature of 170°C for 36 hours, cooled to room temperature, and the reaction product was centrifuged, acid-washed and vacuum-dried to prepare a Pt3Ni / C catalyst.

[0066] Comparative Example 4

[0067] In this comparative example, no vacuum heating or molecular cross-linking agent was used in the preparation process of the catalyst, and the other experimental steps were the same as those in Example 4:

[0068] 1700 mg of acetylene black was slowly added to a mixed solution of 3600 mg of platinum acetylacetonate, 2900 mg of copper acetate and 2000 ml of N,N-dimethylformamide, and ultrasonically treated for 4 hours at normal pressure; finally, the mixed solution was added to an autoclave, reacted at a temperature of 160°C for 48 hours, cooled to room temperature, and the reaction product was centrifuged, washed, vacuum dried, and acid-washed to prepare a Pt3Co / C catalyst.

[0069] Comparative Example 5

[0070] The only difference between the preparation method of the fuel cell oxygen reduction catalyst described in this comparative example and that in Example 1 is that the Ketjen Black EC-300J is not subjected to vacuum heating in step (1).

[0071] Comparative Example 6

[0072] A method for preparing a fuel cell oxygen reduction catalyst comprises the following steps:

[0073] (1) A quartz bottle containing 1000 mg of Ketjen Black EC-300J was placed in a vacuum device with heating and ultrasound, evacuated to a vacuum degree of 100 Pa using a mechanical pump and a molecular pump, and heated to 320°C and kept warm for 3 h.

[0074] (2) A mixed solution of 1200 mg of chloroplatinic acid, 700 mg of cobalt chloride hexahydrate and 600 ml of ethylene glycol was then injected into a quartz bottle containing 1000 mg of Ketjen Black EC-300J in a vacuum chamber using a peristaltic pump at a rate of 45 ml / min. The mixture was then ultrasonically treated with an ultrasonic rod under vacuum conditions for 30 seconds every 1 minute for a total of 3 minutes to completely wet the pores of the Ketjen Black EC-300J. The vacuum was then removed from the quartz bottle containing the mixed solution and ultrasonicated for 30 minutes at room temperature and pressure.

[0075] (3) Finally, the mixed solution was added into an autoclave, reacted at 150°C for 12 hours, cooled to room temperature, and the reaction product was centrifuged, acid-washed, and then vacuum-dried to prepare a Pt3Co / C catalyst.

[0076] Comparative Example 7

[0077] A method for preparing a fuel cell oxygen reduction catalyst comprises the following steps:

[0078] (1) A quartz bottle containing 1000 mg of Ketjen Black EC-300J was placed in a vacuum device with heating and ultrasound, evacuated to a vacuum degree of 100 Pa using a mechanical pump and a molecular pump, and heated to 320°C and kept warm for 3 h.

[0079] (2) A mixed solution of 1200 mg chloroplatinic acid, 700 mg cobalt chloride hexahydrate, 500 mg phenol and 600 ml ethylene glycol was then injected into a quartz bottle containing 1000 mg Ketjen Black EC-300J in a vacuum chamber at a rate of 45 ml / min using a peristaltic pump. The mixture was then ultrasonically treated with an ultrasonic rod under vacuum conditions for 30 seconds every 1 minute for a total of 3 minutes to completely wet the pores of the Ketjen Black EC-300J. The vacuum was then removed from the quartz bottle containing the mixed solution and ultrasonicated for 30 minutes at room temperature and pressure.

[0080] (3) Finally, the mixed solution was added into an autoclave, reacted at 150°C for 12 hours, cooled to room temperature, and the reaction product was centrifuged, acid-washed, and then vacuum-dried to prepare a Pt3Co / C catalyst.

[0081] Effect Example 1

[0082] The morphology and structure of the catalyst materials prepared in Examples 1-3 and Comparative Example 2 were analyzed.

[0083] according to Figure 2-4 It can be seen that Pt3Co nanoparticles and Pt3Ni nanoparticles are uniformly dispersed in the pores of the carbon material without obvious agglomeration, and the average particle size is about 4 nm.

[0084] according to Figure 5 It can be seen that the shapes of the Pt3Co alloy nanoparticles in the Pt3Co / C catalyst prepared in Comparative Example 2 are all spherical, and the spherical shape is the path with the lowest free energy for nucleation and growth of Pt3Co alloy nanoparticles, which also indicates that the Pt3Co alloy nanoparticles nucleate and grow on the carbon surface. In the Pt3Co / C catalyst prepared in Example 2, two typical Pt3Co alloy nanoparticles confined by the graphite carbon layer (marked in the rectangular box) did not grow into spheres but other irregular shapes, which indicates that the Pt3Co alloy nanoparticles are in-situ grown in the carbon pores and confined by the carbon pores.

[0085] according to Figure 6 It can be seen that the XRD diffraction peak positions of the Pt3Co / C catalyst are approximately at 40°, 47°, 69° and 83°, and the positions of these diffraction peaks correspond to the diffraction peak positions of the (111), (200), (220) and (311) crystal planes of the face-centered cubic (fcc) structure of Pt metal (JCPDS04-0802). Further comparing the positions of these peaks with the diffraction peak positions of the standard single metal Pt, the diffraction peak positions are obviously shifted to higher angles, indicating that the face-centered cubic lattice spacing of Pt metal in Pt3Co / C is contracted. This is because the atomic radius of Co is larger than that of Pt, and Co enters the Pt lattice, resulting in a contraction of the lattice spacing, which also proves that Co enters the Pt lattice to form a Pt3Co alloy.

[0086] Effect Example 2

[0087] This effect example evaluates the electrochemical performance of the catalysts prepared in Examples 1-4 and Comparative Examples 1-7.

[0088] 2.5 mg of the catalysts prepared in Examples 1-4 and Comparative Examples 1-7 were weighed respectively, and then deionized water, isopropanol and Nafion solution were added, mixed by ultrasonication, and prepared into 2.5 mL of catalyst ink. 10 μL of ink was dropped on a rotating disk electrode with a diameter of 5 mm. The linear sweep voltammetry (LSV) curve of the catalyst was tested in an O2-saturated 0.1 M HClO4 solution, and the mass activity (MA) of the Pt-based catalyst was calculated to evaluate its initial oxygen reduction (ORR) activity. An accelerated durability test (ADT3W) was performed after 30,000 cycles at a low potential (0.6-0.95 V vs. RHE). The ORR activity before and after the cycle was tested and the loss rate of the activity was calculated to evaluate the durability of the catalyst at a low potential. An accelerated durability test (ADT5K) was performed after 5,000 cycles at a high potential (1.0-1.5 V vs. RHE). The ORR activity before and after the cycle was tested and the loss rate of the activity was calculated to evaluate the durability of the catalyst at a high potential. The test results are shown in Table 1.

[0089] Table 1

[0090]

[0091] According to Table 1 and Figure 7-11It can be seen that the catalysts prepared in Examples 1-4 have higher ORR activity under acidic conditions than the catalysts prepared in Comparative Example 1. After the catalysts prepared in Examples 1-4 were cycled at a low potential (0.6-1.0V) for 30,000 cycles, the ORR activity loss rates were 5.61%, 8.86%, 6.35% and 3.65%, respectively, while the catalysts prepared in Comparative Examples 1-4 were cycled at a low potential (0.6-1.0V) for 30,000 cycles, and the ORR activity loss rates were 30.01%, 27.98%, 37.62% and 32.75%. By comparing the ORR activity loss, it can be seen that the ORR activity loss rate of the catalyst prepared in Example 1-4 is significantly lower than that of the catalyst prepared in Comparative Example 1-4, indicating that the catalyst prepared in Example 1-4 has good durability under low potential cycles.

[0092] The ORR activity loss rates of the four catalysts prepared in Examples 1-4 under high potential (1.0-1.5V) cycles were 19.56%, 23.84%, 11.97% and 3.98%, respectively, and the ORR activity loss rates of the catalysts prepared in Comparative Examples 1-4 were 43.60%, 36.32%, 38.42% and 45.95%, respectively. It can be seen that the ORR activity loss rates of the four catalysts prepared in Examples 1-4 after high potential cycles are significantly lower than the ORR activity loss rates of the catalysts prepared in Comparative Examples 1-4, indicating that the catalysts prepared in the examples have better high potential cycle durability.

[0093] Compared with Example 1, the initial activity of Comparative Example 5 is slightly higher than that of Example 1, but the durability of Comparative Example 5 is significantly worse than that of Example 1. In Comparative Example 5, because the porous carbon carrier is not pre-vacuum heated and exhausted, the metal ions cannot completely enter the pores of the porous carbon, resulting in the growth of metal nanoparticles mainly on the carbon surface without in-situ growth in the carbon pores. Although the synthesized catalyst has a high initial ORR activity, due to the lack of confinement of the metal nanoparticles in the carbon pores, the catalyst has a large ORR activity loss rate and poor durability after 30,000 cycles at low potential (0.6-1.0V) or 5,000 cycles at high potential (1.0-1.5V).

[0094] Compared with Example 1, the initial ORR and durability of Comparative Example 6 are significantly lower than those of Example 1. Although the porous carbon carrier of Comparative Example 6 is vacuum heated and exhausted, so that the metal ions in the solution can enter the pores of the porous carbon. However, since Comparative Example 6 does not carry out the self-assembly process of the cross-linking agent molecules on the carbon, some metal ions are not adsorbed on the carbon, and the growth of the metal nanoparticles is not constrained, resulting in a larger nanoparticle size. The initial ORR activity of the synthesized catalyst is low, and after 30,000 cycles at low potential (0.6-1.0V) or 5,000 cycles at high potential (1.0-1.5V), the ORR activity loss rate of the catalyst is poor.

[0095] Compared with Example 1, the initial ORR activity of Example 7 is similar to that of Example 1, but the durability of Example 7 is poor. In Example 7, the crosslinker molecules and metal ions are first mixed ultrasonically and then enter the carbon pores. The crosslinker molecules coordinated by metal ions can enter the carbon pores, but cannot be anchored in the pores. In addition, in the metal reduction stage, the crosslinker molecules only play the role of protective agents to limit the growth of nanoparticles. The metal atoms first nucleate and grow to form nanoparticles, and then deposit on carbon, resulting in many metal nanoparticles not growing in the carbon pores, but distributed on the carbon surface. Therefore, although the catalyst synthesized in Example 7 has a high initial ORR activity, after 30,000 cycles of low potential (0.6-1.0V) or 5,000 cycles of high potential (1.0-1.5V), the ORR activity loss rate of the catalyst is higher than that of Example 1.

[0096] In summary, the reason why the catalyst prepared in the embodiment has higher low-potential and high-potential cycle durability is mainly due to the in-situ growth of Pt and Pt alloy nanoparticles in the pores of the porous carbon material. The catalyst prepared enables the fuel cell to operate for a long time in the normal working potential range (0.6-0.95V). The carbon pores confine the metal nanoparticles, which enhances the anchoring of the porous carbon carrier to the metal nanoparticles, prevents the agglomeration, dissolution and shedding of the Pt-based alloy nanoparticles in the catalyst, and significantly improves the durability of the Pt-based catalyst at the cathode of the fuel cell. Moreover, the confinement of the metal nanoparticles by the carbon pores also slows down the high-potential (1.0-1.5V) corrosion of the carbon carrier, prevents the collapse of the porous carbon structure, thereby inhibiting the agglomeration, dissolution and shedding of the Pt-based alloy nanoparticles in the catalyst, and significantly improves the durability of the Pt-based catalyst at the cathode of the fuel cell. The catalyst prepared by in-situ growth of Pt and Pt alloy nanoparticles in the porous carbon internal pores prepared by the method of the present invention is very effective in improving the durability of the catalyst at low and high potentials, and can solve the problem of poor durability of fuel cell ORR catalysts when operating at low and high potentials.

[0097] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a fuel cell oxygen reduction catalyst, characterized in that: The steps include: (1) placing the porous carbon material in a vacuum environment, heating and keeping the temperature to remove residual gas, and then cooling; (2) adding a molecular crosslinking agent to an organic solvent, stirring and ultrasonicating to obtain a crosslinking agent mixed solution, then dropping the crosslinking agent mixed solution onto the porous carbon material under a vacuum environment, and after the crosslinking agent mixed solution completely submerges the porous carbon material, ultrasonicating under vacuum negative pressure and ultrasonicating under normal temperature and pressure in sequence to obtain a porous carbon-molecular crosslinking agent-organic solvent mixed solution; (3) Adding a Pt salt solution or a PtM precursor solution composed of a Pt salt and a transition metal salt into a mixed solution of porous carbon-molecular crosslinking agent-organic solvent, mixing and ultrasonicating, and then hydrothermally reacting or hydrogen reduction heat treatment, and finally washing, separating, and vacuum drying to obtain a Pt / C catalyst or a PtM / C catalyst.

2. The method for preparing the fuel cell oxygen reduction catalyst according to claim 1, characterized in that: In the steps (1) and (2), the vacuum degree of the vacuum environment is 100 Pa to 10 -3 Pa; in the step (1), the heating temperature is 50-350°C and the insulation time is 0.5-5h.

3. The method for preparing a fuel cell oxygen reduction catalyst according to claim 1, characterized in that: In the step (2), the molecular cross-linking agent is at least one of phenol, benzoic acid, phenylacetic acid, methyl benzoate, ethyl benzoate, naphthoic acid, naphthoacetic acid, methyl naphthoate, ethyl naphthoate, anthracenecarboxylic acid, anthraceneacetic acid, methyl anthracenecarboxylate, and ethyl anthracenecarboxylate; and the organic solvent is one of ethanol, ethylene glycol, methanol, benzyl alcohol, chloroform, oleic acid, oleylamine, and N,N-dimethylformamide.

4. The method for preparing a fuel cell oxygen reduction catalyst according to claim 1, characterized in that: In the step (2), the concentration of the molecular cross-linking agent in the organic solvent is 0.1 to 10 g / L.

5. The method for preparing a fuel cell oxygen reduction catalyst according to claim 1, characterized in that: In the step (2), ultrasonic treatment is performed for 10 to 30 seconds every 1 to 2 minutes under vacuum negative pressure, for a total of 3 to 120 minutes; and ultrasonic treatment is performed for 0.5 to 10 hours at normal temperature and pressure.

6. The method for preparing a fuel cell oxygen reduction catalyst according to claim 1, characterized in that: In the step (3), the Pt salt is one of platinum acetate, platinum acetylacetonate, chloroplatinic acid, and platinum dichloride; the transition metal salt is one of nickel chloride hexahydrate, nickel acetylacetonate, nickel acetate, cupric chloride dihydrate, copper acetylacetonate, cupric acetate, cobalt chloride hexahydrate, cobalt acetylacetonate, cobalt acetate, ferric chloride hexahydrate, ferric acetylacetonate, and ferric acetate.

7. The method for preparing a fuel cell oxygen reduction catalyst according to claim 1, characterized in that: In the step (3), the concentration of the Pt salt in the Pt salt solution is 2 to 20 g / L; the concentration of the metal ions in the PtM precursor mixed solution is 0.5 to 30 g / L.

8. The method for preparing a fuel cell oxygen reduction catalyst according to claim 1, characterized in that: The mass volume ratio of the porous carbon material to the PtM precursor mixed solution is 0.2-100 g / L: 0.2-100 g / L; the mass volume ratio of the porous carbon material to the Pt salt solution is 0.1-50 g / L: 0.1-50 g / L.

9. The method for preparing a fuel cell oxygen reduction catalyst according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 150-200° C. and the time is 5-60 hours.

10. The method for preparing a fuel cell oxygen reduction catalyst according to claim 1, characterized in that: The temperature of the hydrogen reduction heat treatment is 400-900° C., the time is 1-5 hours, the gas is a mixture of nitrogen and hydrogen or a mixture of argon and hydrogen, the volume ratio of nitrogen to hydrogen in the mixture of nitrogen and hydrogen is 2-10:1, the volume ratio of argon to hydrogen in the mixture of argon and hydrogen is 2-10:1, and the flow rate of the mixed gas is 10-1000 mL / min.

Citation Information

Cited By

  • In-situ etching-micro-crystallization treatment carbon carrier supported catalyst and preparation method thereof