Surface treatment agent
Patent Information
- Application Number
- CN202380024223.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-15
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing technology, the hydrophilic treatment agent used in heat exchangers is difficult to maintain high hydrophilicity and corrosion resistance after long-term use, and at the same time, there is a problem of poor odor suppression effect.
Use a surface treatment agent composed of water-soluble inorganic oxides and their salts, hydrolysates and condensates of organic alkoxysilane, water-soluble resins and ether compounds, and prepare them in appropriate proportions to form a coating with excellent corrosion resistance and hydrophilicity. Film to suppress odor.
It achieves the formation of a coating film with excellent corrosion resistance and hydrophilicity on the surface of the heat exchanger, improves heat exchange efficiency, reduces water droplet retention, extends the service life of the equipment, and suppresses the generation of odor.
Smart Images

Figure BDA0005015846320000151 
Figure BDA0005015846320000161 
Figure BDA0005015846320000171
Abstract
Description
Technical Field
[0001] The present invention relates to a surface treatment agent, and in particular to a surface treatment agent for a metal material. Further, the present invention relates to a surface treatment method for a metal material using the surface treatment agent, a method for manufacturing a surface-treated metal material, a heat exchanger using the surface-treated metal material, a surface treatment method for a heat exchanger, a method for manufacturing a surface-treated heat exchanger, and a surface-treated heat exchanger. Background Art
[0002] In the past, heat exchangers used in air conditioners or motor vehicle air conditioners were mostly made of metal materials, especially aluminum-containing metal materials, due to their advantages in processability and thermal conductivity. In order to improve the heat exchange efficiency, the spacing between the metal materials (usually called heat sinks) in the ventilation area is designed to be very narrow. When the air conditioner is running (cooling), the moisture in the atmosphere condenses on the heat sink and causes condensation, but the higher the hydrophobicity of the heat sink surface, the easier it is for the condensed water to form water droplets, and blockage is likely to occur between the heat sinks. If blockage occurs, the ventilation resistance increases, the heat exchange efficiency decreases, and the original performance of the heat exchanger cannot be obtained. In addition, the noise during air supply sometimes increases due to blockage. In order to solve these problems, a method of imparting hydrophilicity to metal materials has been proposed and implemented.
[0003] As methods for imparting hydrophilicity, hydrophilizing agents having inorganic substances as the main component (hereinafter referred to as inorganic hydrophilizing agents) (see Patent Document 1), hydrophilizing agents having polyacrylamide, polyvinyl alcohol, polyvinyl pyrrolidone, polyacrylic acid and other resins or organic substances as the main component (hereinafter referred to as organic hydrophilizing agents), etc. (see Patent Document 2) have been proposed and implemented.
[0004] Here, the metal material or heat exchanger that is given hydrophilicity by using an inorganic hydrophilizing agent can maintain high hydrophilicity for a long time and has excellent durability, but on the other hand, there is a problem of generating odors such as the coating film odor peculiar to inorganic substances (the odor of dust, hereinafter referred to as dust odor). On the other hand, when an organic hydrophilizing agent is used, although the problem of dust odor is reduced, the organic matter as the hydrophilic component is easy to flow away, and it is difficult to maintain high hydrophilicity for a long time, and there is a durability problem. In order to improve these problems, a hydrophilizing agent is proposed that improves the dust odor peculiar to silica by dispersing silica particles as an inorganic substance using polyvinyl alcohol (see patent document 3). In addition, a hydrophilizing agent based on an alkaline silicate, a specific acrylamide copolymer and a silane coupling agent is proposed (see patent document 4).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 59-13078
[0008] Patent Document 2: Japanese Patent Application Publication No. 2000-328038
[0009] Patent Document 3: Japanese Patent Application Publication No. 2001-323250
[0010] Patent Document 4: Japanese Patent Application Laid-Open No. 1-249863 Summary of the invention
[0011] Problems to be solved by the invention
[0012] However, the coating films based on the hydrophilic treatment agent described in Patent Documents 3 to 4 have excellent odor suppression, but according to the research results of the inventors of the present invention, the organic matter in the hydrophilic coating film formed by the hydrophilic treatment agent flows away due to the long-term use of the air conditioner, and it is not possible to obtain comprehensive excellent performance from the perspectives of odor suppression, corrosion resistance and hydrophilicity. In particular, there is still room for improvement in pitting corrosion resistance (inhibition of perforation corrosion).
[0013] The present invention is developed in view of the above situation, and in one embodiment, its purpose is to provide a surface treatment agent that can form a coating film with excellent corrosion resistance and hydrophilicity and suppressed odor. In addition, in another embodiment of the present invention, its purpose is to provide a surface treatment method of a metal material, a method for manufacturing a surface-treated metal material, a heat exchanger using the surface-treated metal material, a surface treatment method of a heat exchanger, a method for manufacturing a surface-treated heat exchanger, and a surface-treated heat exchanger.
[0014] Means used to solve problems
[0015] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems and have found that preparing one or more selected from the following water-soluble inorganic oxides and their salts (A), one or more selected from the hydrolyzates and condensates of organic alkoxysilanes (B), a water-soluble resin (C) and an ether compound (D) in an appropriate ratio is beneficial for obtaining a surface treatment agent capable of forming a coating film having excellent corrosion resistance and hydrophilicity and suppressed odor, thereby completing the present invention.
[0016] The present invention is exemplarily defined as follows.
[0017] [1] A surface treatment agent comprising one or more selected from water-soluble inorganic oxides and salts thereof (A), one or more selected from hydrolyzates and condensates of organoalkoxysilanes (B), a water-soluble resin (C), an ether compound (D), and water and / or a water-miscible solvent,
[0018] If M A 、M B 、M C and M D represents the total mass of one or more selected from water-soluble inorganic oxides and salts thereof (A), the total mass of one or more selected from hydrolyzates and condensates of organoalkoxysilanes (B), the mass of the water-soluble resin (C) and the mass of the ether compound (D), then (M A +M B ) / (M A +M B +M C +M D )=0.01~0.7.
[0019] [2] A surface treatment agent according to [1], wherein one or more selected from the water-soluble inorganic oxides and their salts (A) are alkaline and contain an element (M1) selected from Si, V, Zr, Mo, Ti and W and a cationic component (M2) selected from Na, K, Li and NH4, and the molar ratio (M2) to (M1) is 0.1 to 8.0.
[0020] [3] A surface treatment agent according to [1] or [2], wherein one or more selected from the water-soluble inorganic oxides and their salts (A) are represented by a molecular formula of the general formula Me2O·nSiO2, Me is a cationic component selected from Na, K, Li and NH4, and n is 0.5 to 8.0.
[0021] [4] The surface treatment agent according to any one of [1] to [3], wherein when M A 、M B represents the total mass of one or more selected from the water-soluble inorganic oxides and salts thereof (A) and the total mass of one or more selected from the hydrolyzates and condensates of the organoalkoxysilane (B), then (M A ) / (M B )=0.25~4.0.
[0022] [5] A surface treatment agent according to any one of [1] to [4], wherein one or more selected from the water-soluble inorganic oxides and their salts (A) form a complex with one or more selected from the hydrolyzates and condensates of the organic alkoxysilane (B), and the median particle size of the complex measured by dynamic light scattering is less than 10 nm.
[0023] [6] The surface treatment agent according to any one of [1] to [5], wherein the water-soluble resin (C) comprises one or more selected from water-soluble resins having one or more functional groups selected from amide groups, hydroxyl groups and carboxyl groups, or water-soluble resins having amide bonds in their skeletons.
[0024] [7] The surface treatment agent according to any one of [1] to [6], wherein when M A 、M B 、M C and M D represents the total mass of one or more selected from the water-soluble inorganic oxides and salts thereof (A), the total mass of one or more selected from the hydrolyzates and condensates of the organoalkoxysilane (B), the mass of the water-soluble resin (C), and the mass of the ether compound (D), then M D / (M A +M B +M C +M D )=0.001~0.2.
[0025] [8] A method for treating a metal material surface, comprising the step of bringing the surface treatment agent according to any one of [1] to [7] into contact with the metal material and then drying the contacted metal material.
[0026] [9] A method for producing a surface-treated metal material, comprising the step of bringing the surface treatment agent according to any one of [1] to [7] into contact with a metal material and then drying the contacted metal material.
[0027]
[10] A heat exchanger using the surface-treated metal material obtained by the manufacturing method according to [9].
[0028]
[11] A method for treating the surface of a heat exchanger, comprising the step of bringing the surface treatment agent according to any one of [1] to [7] into contact with the heat exchanger and then drying the contacted surface.
[0029]
[12] A method for producing a surface-treated heat exchanger, comprising the step of bringing the surface treatment agent according to any one of [1] to [7] into contact with a heat exchanger and then drying the contacted surface.
[0030]
[13] A surface treatment heat exchanger, wherein the surface treatment heat exchanger is obtained by the manufacturing method according to
[12] .
[0031] Effects of the Invention
[0032] According to one embodiment of the present invention, a surface treatment agent can be provided that can form a coating film having excellent corrosion resistance and hydrophilicity and suppressed odor. Therefore, the present invention can help improve the performance of, for example, a heat exchanger having a metal material, especially an air conditioner having a metal material as a heat sink. DETAILED DESCRIPTION
[0033] Hereinafter, an embodiment of the present invention including a surface treatment agent and a surface-treated metal material is described in detail. It should be noted that the present invention can be arbitrarily changed within the scope of the present invention and is not limited to the following embodiments. It should be noted that the "to" indicating a numerical range in this specification also includes an upper limit and a lower limit. For example, "X to Y" means greater than X and less than Y.
[0034] <1. Surface treatment agent>
[0035] According to one embodiment of the present invention, a surface treatment agent is provided, which contains one or more selected from water-soluble inorganic oxides and their salts (A), one or more selected from hydrolyzates and condensates of organic alkoxysilanes (B), a water-soluble resin (C), an ether compound (D), and water and / or a water-miscible solvent.
[0036] [1-1. Water-soluble inorganic oxides and salts thereof (A)]
[0037] One or more selected from water-soluble inorganic oxides and their salts (A) play the role of imparting hydrophilicity and corrosion resistance to the coating film. By being mixed in the coating film, excellent hydrophilicity and corrosion resistance can be ensured for a long time. One water-soluble inorganic oxide and its salt (A) can be used alone or in combination of two or more. One or more selected from water-soluble inorganic oxides and their salts (A) are alkaline, containing an element (M1) selected from Si, V, Zr, Mo, Ti and W and a cationic component (M2) selected from Na, K, Li and NH4, and the molar ratio (M2) / (M1) of (M2) to (M1) is 0.1 to 8.0. When (M2) / (M1) is 0.1 or more, it is possible to prevent the corrosion effect on metals such as aluminum from becoming larger, and the durability of the coating film can be improved. The lower limit of (M2) / (M1) is more preferably 0.5 or more, and further more preferably 1.0 or more. When (M2) / (M1) is 8.0 or less, the water solubility becomes high, and the liquid stability of the surface treatment agent can be improved. By being water-soluble, the advantage of improved processability can be obtained. The upper limit of (M2) / (M1) is more preferably 7.0 or less, and further more preferably 6.0 or less.
[0038] In order to obtain excellent hydrophilicity and corrosion resistance, it is preferred to use an alkaline silicate represented by a molecular formula of the general formula Me2O·nSiO2 (Me represents a cation component selected from Na, K, Li and NH4, and n is 0.5 to 8.0) as one or more selected from water-soluble inorganic oxides and salts thereof (A). It is particularly preferred to use an alkaline silicate having n=1.0 to 8.0.
[0039] It should be noted that, in this specification, "water-soluble" means a substance having a solubility of 0.1% by mass or more in water at room temperature 20°C, preferably 0.5% by mass or more, and more preferably 1% by mass or more. In addition, in this specification, an oxide refers to a compound having a portion in which a metal atom is directly bonded to an oxygen atom and the oxidation number of the metal atom is (+1) or more.
[0040] The fact that one or more selected from the water-soluble inorganic oxides and salts thereof (A) are "alkaline" means that (A) exhibits "alkalinity" when dissolved in water at 25°C at a concentration of 0.1 mass%.
[0041] Examples of other silicon compounds that can be used as one or more selected from the water-soluble inorganic oxides and salts thereof (A) include hydrates of silicon dioxide.
[0042] Examples of the titanium compound that can be used as one or more selected from the water-soluble inorganic oxides and salts thereof (A) include salts of titanium oxide (potassium, ammonium salts, etc.).
[0043] Examples of the vanadium compound that can be used as one or more selected from the water-soluble inorganic oxides and salts thereof (A) include vanadates (sodium, potassium, ammonium salts, etc.), metavanadates (sodium, potassium, ammonium salts, etc.), and the like.
[0044] Examples of the zirconium compound that can be used as one or more selected from the water-soluble inorganic oxides and salts thereof (A) include zirconium carbonate and its hydrate, and zirconium carbonate salts such as ammonium zirconium carbonate and potassium zirconium carbonate.
[0045] Examples of the molybdenum compound that can be used as one or more selected from the water-soluble inorganic oxides and salts thereof (A) include molybdic acid and salts thereof (sodium, potassium, ammonium salts, etc.).
[0046] Examples of the tungsten compound that can be used as one or more selected from the water-soluble inorganic oxides and salts thereof (A) include salts of tungstic acid (sodium, potassium, ammonium salts, etc.).
[0047] [1-2. Hydrolyzate and condensate of organoalkoxysilane (B)]
[0048] One or more selected from the hydrolyzates and condensates of the organoalkoxysilane (B) are mixed in the coating film, which can reduce the dust odor peculiar to the water-soluble inorganic oxide and its salt (A). In addition, it acts as a binder of the coating film constituent component, inhibits the flow of the water-soluble inorganic oxide and its salt (A), the water-soluble resin (C) and the ether compound (D), and helps to show hydrophilicity, corrosion resistance and odor suppression for a long time. Furthermore, it also helps to ensure the stability of the water-soluble inorganic oxide and its salt (A) in the surface treatment agent, and improves the stability of the treatment agent.
[0049] One or more selected from the hydrolyzate and condensate of the organoalkoxysilane (B) are not particularly limited as long as they can be hydrolyzed or dehydrated and condensed in water. The organoalkoxysilane (B) may be used alone or in combination of two or more.
[0050] As an organic alkoxysilane, for example, a silane coupling agent having an alkoxy group as a hydrolyzable group can be cited. As an alkoxy group, there is no limitation, and examples thereof include alkoxy groups having 1 to 4 (especially 1 or 2) carbon atoms such as methoxy, ethoxy, propoxy, butoxy, etc. In addition, the silane coupling agent can have, for example, an epoxy group (especially a glycidyl group), an amino group, a vinyl group, a mercapto group, an acryloxy group, a methacryloxy group, a urea group, an isocyanate group, etc. as an organic functional group. Among them, based on the excellent aspect of the composite with a water-soluble inorganic oxide and its salt (A), it is preferably selected from one or more organic alkoxysilanes having one or more glycidyl groups as organic functional groups. As a preferred organic alkoxysilane, for example, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldiethoxysilane can be cited. Unless otherwise indicated, the organoalkoxysilane may have one or more amino groups, vinyl groups, mercapto groups, acryloyloxy groups, methacryloyloxy groups, urea groups, or isocyanate groups in addition to the glycidyl group.
[0051] Organic alkoxysilane is hydrolyzed in water to generate silanol and alcohol as hydrolyzates. Sometimes the silanol and / or alcohol generated by hydrolysis can form hydrogen bonds with each other, but in this specification, such substances are also treated as hydrolyzates. Furthermore, a part or all of the silanol generated by hydrolysis undergoes a dehydration condensation reaction, and sometimes a condensation reaction product (organic siloxane) having a siloxane bond (Si-O-Si) can also be generated. Therefore, the surface treatment agent involved in the present invention contains one or more selected from the hydrolyzate and condensate of the organic alkoxysilane (B).
[0052] [1-3. Water-soluble resin (C)]
[0053] The water-soluble resin (C) is mixed in the coating film, and it is believed that it inhibits the complex of the water-soluble inorganic oxide and its salt (A) and the organic alkoxysilane (B) from flowing out of the coating film system in flowing water or corrosive environment, thereby improving the durability of the coating film and helping to continuously show corrosion resistance, hydrophilicity and odor resistance. Among the water-soluble resins (C), water-soluble resins having one or more functional groups selected from amide groups, hydroxyl groups and carboxyl groups, or water-soluble resins having amide bonds in the skeleton are preferred. The water-soluble resins (C) can be used alone or in combination of two or more.
[0054] As preferred examples of the water-soluble resin (C) having an amide group, for example, homopolymers and copolymers of acrylamide compounds can be cited. As acrylamide compounds, (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, N-methylenesulfonic acid acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, etc. can be cited. As copolymers, copolymers of one or more acrylamide monomers and one or more other comonomers can be exemplified. When manufacturing the copolymer, it is preferred to polymerize at a molar ratio of acrylamide monomer: comonomer = 95:5 or less, more preferably at a molar ratio of 90:10 to 10:90, and even more preferably at a molar ratio of 85:15 to 15:85. The comonomer used here is selected from anionic, nonionic, and cationic addition polymerization monomers that can be polymerized with acrylamide compounds, for example, anionic unsaturated monomers such as (meth)acrylic acid, itaconic acid, maleic acid, vinyl sulfonic acid, styrene sulfonic acid, sulfoethyl acrylate, sulfoethyl methacrylate, phosphooxyethyl methacrylate or its salts; nonionic unsaturated monomers such as hydroxyethyl hydroxy(meth)acrylate, vinyl pyrrolidone, acryloylmorpholine, polyethylene glycol acrylate, polyethylene glycol acrylate alkylphenyl ether; and cationic unsaturated monomers such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl acrylate, N-hydroxypropylaminoethyl (meth)acrylate, hydroxymethylaminoethyl methacrylate, vinylimidazole, vinylpyridine, N,N-diallylamine, N,N-diallyl-N,N-dimethylammonium chloride, etc.
[0055] From the viewpoint of improving the durability of the coating film, the weight average molecular weight of the water-soluble resin (C) having an amide group, particularly a homopolymer and copolymer of an acrylamide compound, is preferably 5,000 to 2,000,000, and more preferably 5,000 to 1,500,000.
[0056] As a water-soluble resin (C) having a hydroxyl group, a water-soluble resin with a high hydroxyl density is preferred based on long-term hydrophilicity and odor resistance, and polyvinyl alcohol or a derivative thereof is more preferred. Polyvinyl alcohol or a derivative thereof means a polymer containing (-CH2CH(OH)-) repeating units, which can be manufactured according to a known method without particular limitation. For example, examples thereof include partially saponified and completely saponified polyvinyl esters obtained by free radical polymerization of vinyl esters as monomers, partially saponified and completely saponified copolymers of vinyl esters and other comonomers, and modified products of polyvinyl alcohol. As vinyl esters, examples thereof include vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl versatate, and vinyl caproate. Among them, vinyl acetate is preferred.
[0057] The comonomers copolymerized with the vinyl ester are not particularly limited, for example, α-olefins such as ethylene or propylene; α-olefins containing hydroxyl groups such as 3-butene-1-ol, 4-pentene-1-ol, 5-hexene-1,2-diol and their derivatives such as acylates; unsaturated acids such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, their salts, their monoalkyl esters or dialkyl esters; nitriles such as acrylonitrile; amides such as methacrylamide and diacetone acrylamide; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, methyl allyl sulfonic acid or their salts; allyl compounds such as ethylene oxide monoallyl ether, etc. These comonomers can be used alone or in combination of two or more. When manufacturing the copolymer, it is preferred to polymerize at a molar ratio of vinyl ester monomer: comonomer = 95:5 or less, more preferably at a molar ratio of 90:10 to 10:90, and even more preferably at a molar ratio of 85:15 to 15:85.
[0058] The saponification degree of polyvinyl alcohol or its derivative is preferably 90 mol% or more, more preferably 95 mol% or more, based on long-term hydrophilicity and odor resistance, and there is no particular upper limit, and it may be 100 mol%. The saponification degree of polyvinyl alcohol or its derivative is measured in accordance with JIS K6726:1994.
[0059] The weight average molecular weight of the water-soluble resin (C) having a hydroxyl group (typically polyvinyl alcohol or its derivatives) is preferably 5,000 to 200,000, and more preferably 5,000 to 100,000, in order to improve the durability of the coating film. In particular, when one or more selected from polyvinyl alcohol or its derivatives and the saponification degree is 90 mol% or more, the weight average molecular weight is more preferably 10,000 to 50,000.
[0060] Suitable examples of the water-soluble resin (C) having a carboxyl group can be exemplified by polyacrylic acid or a derivative thereof.
[0061] Polyacrylic acid or its derivatives refer to polymers containing structures derived from (meth) acrylic acid (salt), which can be manufactured according to known methods without particular restrictions. For example, it is a polymer obtained by subjecting (meth) acrylic acid (salt) to free radical polymerization and a copolymer thereof or its salt. The structure derived from (meth) acrylic acid (salt) is a structure formed by subjecting (meth) acrylic acid (salt) to free radical polymerization, represented by -CH2CR(COOM)-. In this structure, R represents a hydrogen atom or a methyl group, and M represents a hydrogen atom, a metal atom, an ammonium salt or an organic amine salt. As the above-mentioned metal atom, alkali metal atoms such as Li, Na, and K, and alkaline earth metal atoms such as Ca and Mg can be exemplified. The above-mentioned (meth) acrylic acid (salt) represents acrylic acid, acrylic acid salt, methacrylic acid, and methacrylic acid salt, among which acrylic acid and acrylic acid salt are preferred. These (meth) acrylic acid (salts) can be used alone or in combination. As salts in the above-mentioned (meth) acrylic acid (salt), metal salts, ammonium salts, and organic amine salts can be listed. When polyacrylic acid or a derivative thereof is a copolymer, the polymerization is preferably carried out at a molar ratio of (meth)acrylic acid (salt):comonomer=95:5 or less, more preferably at a molar ratio of 90:10 to 10:90, and even more preferably at a molar ratio of 85:15 to 15:85.
[0062] The weight average molecular weight of the homopolymer and copolymer of the water-soluble resin (C) having a carboxyl group (particularly polyacrylic acid or a derivative thereof) is preferably 5,000 to 2,000,000, more preferably 10,000 to 1,000,000, in order to improve the durability of the coating film.
[0063] The water-soluble resin (C) having an amide bond in the skeleton may be, for example, a water-soluble polyamide. Examples of the water-soluble polyamide include basic polyamides obtained from polyalkylene polyamines and aliphatic dicarboxylic acids (such as adipic acid), and epoxy-modified polyamides produced by reacting the basic polyamides with epichlorohydrin. In addition, examples include cationic polyamides containing amino groups or nonionic polyamides containing ethylene oxide.
[0064] The weight average molecular weight of the water-soluble resin (C) in the present invention is measured by GPC method. The weight average molecular weight in Examples is measured under the following conditions.
[0065] <Measurement conditions based on GPC>
[0066] The measurement was performed using a high-speed GPC apparatus (HLC-8320GPC: manufactured by Tosoh Corporation), and the weight average molecular weight was determined using a combination of a SEC column and a guard column. The measurement was performed under the following conditions.
[0067] SEC column: TSKgel SuperAWM-H (manufactured by Tosoh Corporation)
[0068] Guard column: TSKgurdcolumn SuperAW-H (manufactured by Tosoh Corporation)
[0069] Detector: RI (HLC-8320GPC built-in detector)
[0070] Standard sample: polystyrene
[0071] Sample injection volume: 0.06% DMF solution 30 μL
[0072] Flow rate: 0.5mL / min
[0073] Eluent: DMF / 100mM LiBr / 60mM H3PO4
[0074] [1-4. Ether compound (D)]
[0075] The ether compound (D) refers to a compound having an ether bond represented by -COC- in the molecule. The ether compound (D) plays a role in improving hydrophilicity. In addition, although the present invention is not intended to be limited by theory, it can be considered that the ether compound (D) improves the durability of the coating film by inhibiting the flow of the water-soluble resin (C). As the ether compound (D), there is no limitation, and polyalkylene glycol, polyalkylene glycol alkyl ether, polyoxyalkylene alkyl ether, polyoxyalkylene phenyl ether, ether ester compound, glycidyl ether compound and carbohydrate having pyranose structure or furanose structure can be listed. The ether compound (D) can be used alone or in combination of two or more.
[0076] Examples of polyalkylene glycols include polyethylene glycol and polypropylene glycol. Examples of polyalkylene glycol alkyl ethers include polyethylene glycol (mono) methyl ether, poly(ethylene, propylene) glycol (mono) methyl ether, polyethylene glycol (mono) ethyl ether, etc. Examples of polyoxyalkylene alkyl ethers include polyoxyethylene alkyl (especially alkyl having 12 to 15 carbon atoms) ethers. Examples of polyoxyalkylene phenyl ethers include polyoxyethylene phenyl ethers. Examples of ether ester compounds include polyoxyethylene lauryl ether sodium sulfate, polyoxyethylene sorbitol ether fatty acid esters, etc. These polyoxyalkylene alkyl ethers may be ether compounds having multiple alkylene structures having different numbers of carbon atoms.
[0077] Examples of the glycidyl ether compound include sorbitol polyglycidyl ether, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, phenolic glycidyl ether containing ethylene oxide, dodecanol glycidyl ether containing ethylene oxide, bisphenol A type epoxy resin, bisphenol F type epoxy resin, and bisphenol AD type epoxy resin.
[0078] Examples of carbohydrates having a pyranose structure or a furanose structure include polysaccharides such as starch, glycogen, cellulose, chitin, and dextran, and derivatives thereof. Examples of cellulose derivatives as polysaccharide derivatives include alkyl celluloses such as methyl cellulose (MC), hydroxyalkyl celluloses such as hydroxypropyl cellulose (HPC) and hydroxyethyl cellulose (HEC), hydroxyalkyl alkyl celluloses such as hydroxypropyl methyl cellulose (HPMC), hydroxyethyl methyl cellulose (HEMC), and hydroxyethyl ethyl cellulose (HEEC), and sodium carboxymethyl cellulose (CMC-Na).
[0079] [1-5. Other ingredients (E)]
[0080] The surface treatment agent may contain various additives such as acid catalysts, crosslinking agents, antibacterial agents, lubricants, surfactants, pigments, dyes, inhibitors for imparting corrosion resistance, etc. as needed. In addition, in order to dissolve the necessary components, the surface treatment agent preferably contains water, a water-miscible solvent, or a mixed solvent of water and a water-miscible solvent. Based on the viewpoint of easy handling of the surface treatment agent, deionized water is preferably used as water. The content of water is preferably 80 to 99% by mass, more preferably 85 to 95% by mass, relative to the total amount of the surface treatment agent. In the case of using a mixed solvent of water and a water-miscible solvent, the proportion of water, for example, relative to the total mass of the mixed solvent, should preferably be 60% by mass or more. As a water-miscible solvent, as long as it is a solvent that does not phase separate after mixing with water, it is not particularly limited, and for example, alcohols such as methanol and ethanol can be cited.
[0081] The type of the acid catalyst (opening of the epoxy group, hydrolysis of the alkoxy group bonded to silicon) is not particularly limited. For example, as an organic acid, there can be listed (1) carboxylic acids (monocarboxylic acids, dicarboxylic acids, tricarboxylic acids, etc.) such as formic acid, acetic acid, butyric acid, oxalic acid, succinic acid, lactic acid, L-ascorbic acid, tartaric acid, citric acid, DL-malic acid, malonic acid, maleic acid, and phthalic acid, (2) aminotrimethylenephosphonic acid, aminotripropylenephosphonic acid, aminodiethylmethylenephosphonic acid, methane-1-hydroxy-1,1-diphosphonic acid, ethane-1-hydroxy-1,1-diphosphonic acid, propane-1-hydroxy-1,1-diphosphonic acid, (3) sulfonic acids such as methanesulfonic acid and benzenesulfonic acid, and (4) phosphoric acid as an inorganic acid. It should be noted that the acid catalyst also remains in the coating film after the coating film is formed. Based on this, since the obtained coating film has excellent water resistance, it is preferably an organic acid, and more preferably a carboxylic acid. These may be used alone or in combination of two or more.
[0082] [1-6. Mixing ratio (A) to (D)]
[0083] If M A 、M B 、M C and M D represents the total mass of one or more selected from the group consisting of water-soluble inorganic oxides and salts thereof (A), the total mass of one or more selected from the group consisting of hydrolyzates and condensates of organic alkoxysilanes (B), the mass of the water-soluble resin (C), and the mass of the ether compound (D) contained in the surface treatment agent, and is required to satisfy (M A +M B ) / (M A +M B +M C +M D )=0.01~0.7. Furthermore, it is preferred to satisfy (M A +M B ) / (M A +M B +M C +M D )=0.05~0.5, and more preferably satisfy (M A +M B ) / (M A +M B +M C +M D )=0.1~0.4. If (M A +M B ) / (M A +M B +M C +M D) is greater than 0.7, the composite of one or more selected from the group consisting of water-soluble inorganic oxides and salts thereof (A) and one or more selected from the group consisting of hydrolyzates and condensates of organic alkoxysilanes (B) described later cannot be sufficiently fixed in the coating film and flows away, resulting in insufficient hydrophilicity and corrosion resistance. A +M B ) / (M A +M B +M C +M D ) is less than 0.01, the effective ingredients are insufficient and the hydrophilicity and corrosion resistance are insufficient.
[0084] Furthermore, if we use M A 、M B represents the total mass of one or more selected from the group consisting of water-soluble inorganic oxides and salts thereof (A) and the total mass of one or more selected from the group consisting of hydrolyzates and condensates of organic alkoxysilanes (B) contained in the surface treatment agent, preferably satisfies (M A ) / (M B )=0.25~4.0, and more preferably 0.5~2.0. A ) / (M B ) is 4.0 or less, one or more selected from the group consisting of water-soluble inorganic oxides and salts thereof (A) can be easily covered and retained by one or more selected from the group consisting of hydrolyzates and condensates of organic alkoxysilane (B), the odor suppression effect is improved, and the hydrophilicity and corrosion resistance are improved. In addition, (M A ) / (M B ) is 0.25 or more, which can suppress the reduction in stability of one or more selected from the water-soluble inorganic oxides and salts thereof (A) in the surface treatment agent, or the reduction in operability due to precipitation or aggregation caused by long-term storage.
[0085] Furthermore, if we use M A 、M B 、M C and M D represents the total mass of one or more selected from the group consisting of water-soluble inorganic oxides and salts thereof (A), the total mass of one or more selected from the group consisting of hydrolyzates and condensates of organic alkoxysilanes (B), the mass of the water-soluble resin (C), and the mass of the ether compound (D) contained in the surface treatment agent, then preferably M D / (M A +M B +M C +M D )=0.001~0.2, more preferably 0.01~0.2, and even more preferably 0.03~0.2.D / (M A +M B +M C +M D ) is 0.2 or less, which can inhibit the decrease in water resistance of the coating film, improve the corrosion resistance, and easily improve the hydrophilicity during durability. D / (M A +M B +M C +M D ) is 0.001 or more, improvement in hydrophilicity can be expected.
[0086] As described later, one or more selected from the water-soluble inorganic oxides and their salts (A) and one or more selected from the hydrolyzates and condensates of the organic alkoxysilane (B) can react to form a complex, but it is difficult to quantitatively analyze and determine the chemical structure of the complex. A and M B is determined as the mass when no complex is formed in the surface treatment agent. B Since it is difficult to quantitatively analyze and determine the hydrolyzate and condensate, the mass of the raw material organic alkoxysilane (B) is used as the basis for determination. A 、M C and M D , and is determined based on the mass of one or more selected from the water-soluble inorganic oxides and salts thereof (A), the water-soluble resin (C) and the ether compound (D) when they are respectively formulated.
[0087] [1-7. Complex]
[0088] Preferably, one or more selected from water-soluble inorganic oxides and salts thereof (A) and one or more selected from the hydrolyzate and condensate of organic alkoxysilane (B) form a complex in the surface treatment agent. The chemical structure of the complex may not be clear, but it is speculated that the structure formed by the silanol (-Si-OH) produced by the hydrolysis of organic alkoxysilane and the metal element of the water-soluble inorganic oxide and its salt is bonded. In this specification, when a spectroscopic measurement based on multinuclear NMR is performed, when a peak of (Si-O-Me; Me is a metal atom or cationic component that constitutes a water-soluble inorganic oxide and its salt (A) and is directly bonded to an oxygen atom, such as Si, V, Zr, Mo, Ti, W, Na, K, Li or NH4) is observed, it is determined that a complex exists, and when the above-mentioned peak is not observed, it is determined that there is no complex.
[0089] In the Examples, spectroscopy measurement based on multinuclear NMR was performed under the following conditions.
[0090] ·Measurement device: JNM-ECX400 manufactured by JEOL Ltd.
[0091] Probe: NM-40T10AT manufactured by JEOL Ltd.
[0092] Determination solvent: heavy water
[0093] The particle size of the complex of one or more selected from water-soluble inorganic oxides and salts thereof (A) and one or more selected from the hydrolyzate and condensate of organic alkoxysilane (B) contributes to the stability and coating film formation of the surface treatment agent. The smaller the particle size of the complex, the less likely it is to produce precipitation in the treatment agent during long-term storage. By using a surface treatment agent, the adhesion of the coating film and the film forming property of the coating film itself are also easily improved. From the above viewpoint, the median particle size of the complex is preferably less than 10nm.
[0094] The "median particle size" in the present invention refers to the particle size at which 50% of the particles are accumulated, regardless of whether they are primary particles or secondary particles, based on the scattered light intensity when the particle size distribution is measured by the dynamic light scattering method. Examples of measuring equipment for the dynamic light scattering method include UPA-EX150 manufactured by Nikkiso Co., Ltd. The dynamic light scattering method utilizes the fact that the speed of movement (Brownian motion) of particles in a solution varies depending on their size. The solution is irradiated with a laser, and the scattered light is observed using a photon detector, and frequency analysis is performed to obtain the particle size distribution. In the embodiments, the particle size distribution of the composite is measured under the following conditions. In the measurement procedure, although the particle size distribution of particles other than the composite is also included, it is difficult to separate them for measurement. Therefore, in this specification, even if particles other than the composite are present, they are regarded as the particle size distribution of the composite.
[0095] (Particle size measurement conditions)
[0096] Measuring device: UPA-EX150 manufactured by Nikkiso Co., Ltd.
[0097] Light source: semiconductor laser 780nm, 3mW
[0098] Light source probe: internal probe method
[0099] Adjustment of the measurement sample: A complex of one or more selected from the water-soluble inorganic oxides and salts thereof (A) and one or more selected from the hydrolyzates and condensates of the organic alkoxysilane (B) is diluted with deionized water so that the solid content concentration reaches about 0.01% by mass, and then fully stirred and dispersed. It should be noted that the solid content concentration referred to here refers to the value measured according to the normal pressure heating drying method (sample weight: 1.0 g, drying temperature 110°C × 2 hours drying) of JIS K6828-1:2003.
[0100] Measurement time: 180 seconds
[0101] Cycle: None
[0102] Permeability: Permeable
[0103] Shape: Non-spherical
[0104] Refractive index: 1.81 (device default setting)
[0105] Solvent: Water
[0106] Solvent refractive index: 1.333
[0107] [1-8. pH of surface treatment agent]
[0108] The pH (at 25° C.) of the surface treatment agent is preferably 7.0 or higher, more preferably 7.0 to 11.0, and even more preferably 7.0 to 10.0.
[0109] [1-9. Preparation method]
[0110] The surface treatment agent can be prepared by, for example, mixing the above-mentioned components at a desired ratio, adding a required amount of water to the mixture, and stirring the mixture.
[0111] Among them, one or more of the hydrolyzates and condensates selected from the organoalkoxysilane (B) can be generated in water in advance and then mixed with other components, or the organoalkoxysilane (B) can be mixed with other components to generate one or more of the hydrolyzates and condensates during mixing. In any case, in order to efficiently hydrolyze the organoalkoxysilane (B), it is preferably stirred while heating to 30 to 80° C. In order to promote the hydrolysis of the organoalkoxysilane (B), an acid catalyst can be added as needed.
[0112] Furthermore, in order to promote the formation of the complex, before mixing one or more selected from water-soluble inorganic oxides and salts thereof (A) and the organic alkoxysilane (B) with other components, a pre-treatment such as heating and stirring can be performed by placing in a container in water. In order to efficiently hydrolyze the organic alkoxysilane (B), the heating is preferably 30 to 80°C. As another method, before mixing one or more selected from water-soluble inorganic oxides and salts thereof (A) and one or more selected from the hydrolyzate and condensate of the organic alkoxysilane (B) with other components, a pre-treatment such as stirring can be performed by placing in a container in water. It is preferred to heat to 30 to 80°C during the pre-treatment to promote the formation of the complex. In these pre-treatments, an acid catalyst can be added as needed to promote the hydrolysis of the organic alkoxysilane (B).
[0113] <2. Surface treated metal materials and surface treated heat exchangers>
[0114] According to one embodiment of the present invention, a surface treatment method for a metal material and a method for manufacturing a surface-treated metal material are provided, which include: a process of bringing the surface treatment agent into contact with the surface or on the surface of the metal material; and a process of drying the surface treatment agent after the contacting process. In addition, by this manufacturing method, a metal material having a surface treatment coating film can be obtained. The metal material manufactured in this way has a surface treatment coating film on the surface, which is useful for forming a heat dissipation sheet. In addition, the heat dissipation sheet is useful as a component of a heat exchanger. Therefore, according to one embodiment of the present invention, a heat exchanger using the surface-treated metal material obtained by the above-mentioned manufacturing method is provided.
[0115] According to another embodiment of the present invention, a surface treatment method for a heat exchanger and a method for manufacturing a surface-treated heat exchanger are provided, which include: a process of bringing the surface treatment agent into contact with the surface or on the surface of the heat exchanger; and a process of drying the surface treatment agent after the contacting process. In addition, by this method, a surface-treated heat exchanger having a surface-treated coating film can be obtained. The heat exchanger thus obtained has a surface-treated coating film with excellent corrosion resistance, so that the equipment can have a long service life, which is useful in achieving effective utilization of resources. In addition, the surface-treated coating film formed on the heat exchanger is also excellent in hydrophilicity, so water droplets will not be retained between the fins, and the reduction in heat exchange efficiency can be suppressed, which is useful in achieving improved energy efficiency.
[0116] The ratio of one or more selected from water-soluble inorganic oxides and their salts (A), one or more selected from hydrolysates and condensates of organic alkoxysilanes (B), water-soluble resins (C) and ether compounds (D) in the surface treatment coating film is substantially the same as the ratio of one or more selected from water-soluble inorganic oxides and their salts (A), one or more selected from hydrolysates and condensates of organic alkoxysilanes (B), water-soluble resins (C) and ether compounds (D) in the surface treatment agent.
[0117] [2-1. Metal materials and heat exchanger materials]
[0118] The metal material and the material of the heat exchanger to which the above-mentioned surface treatment agent can be applied are not particularly limited, and examples thereof include aluminum, steel, stainless steel, titanium and alloys thereof. The above-mentioned surface treatment agent is particularly suitable for aluminum-containing metal materials. The material constituting the aluminum-containing metal material can be pure aluminum or an aluminum alloy.
[0119] [2-2. Cleaning process]
[0120] Untreated metal materials and heat exchangers are preferably cleaned in advance with an acidic or alkaline cleaning agent. Examples of acidic cleaning agents used include acidic aqueous solutions containing at least one of nitric acid, sulfuric acid, and hydrofluoric acid. Examples of alkaline cleaning agents include alkaline aqueous solutions containing at least one of sodium hydroxide, sodium silicate, and sodium phosphate. In order to improve the cleaning properties, a surfactant may be added to the alkaline aqueous solution. Examples of cleaning methods for metal materials and heat exchangers include immersion methods and spray methods.
[0121] [2-3. Anti-rust treatment]
[0122] After the cleaning process, rust prevention treatment may also be performed. Rust prevention treatment methods include chemical conversion treatment methods and base rust prevention treatment based on resin primers. Among them, as the chemical conversion treatment agent used in the chemical conversion treatment method, it can be listed as a chromic acid chromate treatment agent, a phosphate chromate treatment agent or a non-chromium treatment agent that is well known in the past. As the resin primer, it can be listed as a water-soluble or water-dispersible water-based resin that is well known in the past. As the rust prevention treatment method, for example, it can be listed as an immersion method and a spray method.
[0123] [2-4. Contact process]
[0124] The method of bringing the surface treatment agent into contact with the surface or on the surface of the metal material and the heat exchanger is not particularly limited, and examples thereof include dipping, spraying, roller coating, brushing, etc. The surface treatment agent temperature may be about 10 to 50° C. The contact time may be about 3 seconds to 5 minutes.
[0125] [2-5. Drying process]
[0126] The method for drying the surface treatment agent is not particularly limited as long as the water in the surface treatment agent is evaporated. For example, it can be listed as a drying method using known drying equipment, such as an oven, an intermittent drying furnace, a continuous hot air circulation drying furnace, a crawler hot air drying furnace, an electromagnetic induction heating furnace using an IH heater, etc. The drying temperature can be 100 to 250°C, preferably 120 to 180°C. The drying time can be 10 seconds to 120 minutes, preferably 1 to 60 minutes.
[0127] [2-6. Quality of surface treatment coating film]
[0128] The mass of the metal material having the surface treatment coating film and the surface treatment coating film in the heat exchanger is not particularly limited as long as it can exert the effect of the present invention, but is preferably 0.01 to 5.0 g / m 2 In the range of 0.05 to 3.5 g / m 2 In the range of 0.1 to 2.0 g / m 2 If the surface treatment coating film weight is 0.1g / m 2 The above results in sufficient coating of the metal material and the heat exchanger, and a coating film having excellent hydrophilicity and corrosion resistance and suppressed odor, which is the purpose of the present invention, can be obtained. 2 The following is economical.
[0129] [2-7. Post-processing steps]
[0130] After the surface treatment coating film is formed, a post-treatment process can be implemented. As the post-treatment process, a lubricating oil contact process or a lubricating coating film forming process can be listed. More specifically, it can be listed as a process of making the lubricating oil contact with the surface treatment coating film on the surface of the metal material and the heat exchanger, or contacting the lubricant to form a lubricating coating film. In this way, a metal material and a heat exchanger with a multi-layer coating film formed by contacting the lubricating oil or forming a lubricating coating film on the above-mentioned surface treatment coating film can be obtained. It should be noted that there is no particular limitation on the contact method as the lubricating oil or the lubricant, for example, it can be listed as a roller coating method, a spray method and a dipping method.
[0131] As the lubricating oil, known lubricating oils used during molding can be used. In addition, as the lubricant for forming the lubricating coating film, known lubricants such as water-soluble polyether, polyethylene glycol, polyoxyethylene alkyl ether, polyoxyethylene hardened castor oil ether can be used.
[0132] Example
[0133] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.
[0134] <Synthesis of a complex of one or more selected from water-soluble inorganic oxides and salts thereof (A) and one or more selected from hydrolyzates and condensates of organoalkoxysilanes (B)>
[0135] [Synthesis Examples X1 to X19]
[0136] First, the synthesis method is described by taking Synthesis Example X1 as an example. 49 g of lithium silicate and 49 g of 3-glycidoxypropyltrimethoxysilane, 900 g of deionized water, and 2 g of acetic acid are sequentially added into a glass container equipped with a stirrer, and the ring-opening reaction and the hydrolysis of the methoxy group are started at 60°C. After 2 hours from the start of the reaction, the bath temperature is cooled to below 40°C, and then the water reduced by evaporation is fixed to volume with deionized water to obtain an aqueous dispersion containing a complex of lithium silicate (A1) and one or more selected from the hydrolyzate and condensate of 3-glycidoxypropyltrimethoxysilane (B1), with a solid content of 10% by mass. The concentration of "solid content" mentioned here refers to the value measured by the normal pressure heating drying method (sample weight: 1.0 g, drying temperature 110°C × 2 hours drying) according to JIS K6828-1:2003.
[0137] The composites of Synthesis Examples X2 to X19 were synthesized in the same manner as Synthesis Example X1 except that the inorganic compound (A) and organoalkoxysilane (B) shown in Table 1 and other components (E) shown in Table 3 were used in the amounts shown in Table 1.
[0138] The details of the inorganic compound (A) used in Synthesis Examples X1 to X19 are shown in Table 2. The pH when the inorganic compound (A) was dissolved in water at 25° C. at a concentration of 0.1 mass % is shown in Table 2. The colloidal silica of A6 is water-insoluble.
[0139] The median particle size of the composites of Synthesis Examples X1 to X19 obtained by the above steps was measured by the above-mentioned dynamic light scattering method. The measurement results are shown in Table 1. Due to the analytical precision, values less than 10 nm are marked as "<10". The presence of the composite was confirmed by the above-mentioned multinuclear NMR spectral measurement.
[0140]
[0141] Table 2
[0142]
[0143] Table 3
[0144] Other ingredients (E) Substance name E1 Acetic acid E2 tartaric acid E3 Diisopropyl bis(ethyl acetoacetate) titanate
[0145] <Synthesis of Water-Soluble Resin (C)>
[0146] [Synthesis Example C1]
[0147] In a 2L autoclave reactor equipped with a reflux cooler, a raw material inlet, a thermometer, a pressurized gas inlet, and a stirring blade, 50g of vinyl acetate and 80g of methanol were introduced while introducing nitrogen as a pressurized gas, and 30mL of a 2% by mass methanol solution of 2,2'-azobis(2,4-dimethylvaleronitrile) was added as an initiator in small amounts each time. After adding all the methanol solution, the polymerization reaction was started by heating to 60°C. After 5 hours from the start of the reaction, unreacted vinyl acetate was removed under reduced pressure to prepare a vinyl acetate resin methanol solution. A 10% by mass aqueous sodium hydroxide solution was added to the obtained vinyl acetate resin methanol solution so that the molar ratio of sodium hydroxide to vinyl acetate (50g) used as a raw material was 0.01, and saponification was carried out at 50°C for 1 hour. Then, methanol was removed by distillation under reduced pressure, water was removed by centrifugation, and dried to obtain a powder of polyvinyl alcohol (resin C1) with a saponification degree of 98 mol%. The weight average molecular weight was measured by gel permeation chromatography (GPC) under the above conditions and was 13,000. The ethylene modification rate (the content of ethylene structural units in the water-soluble resin (C)) was measured by proton NMR and was 0 mol%.
[0148] The specific measurement steps of the ethylene modification rate are as follows. Add resin (A) to deionized water and heat to 85-95°C to dissolve it. Dilute it with dimethyl sulfoxide (DMSO)-d6 to a concentration of 1.0% by mass of resin (A) as an NMR sample. Use a nuclear magnetic resonance analyzer (e.g., JNM-EX400: JEOL Ltd.) for proton NMR measurement. The measurement is carried out under the following conditions.
[0149] Detection nuclide: 1H
[0150] Observed temperature: 25.1℃
[0151] Each peak in the obtained spectrum was assigned as follows.
[0152] 1.0 to 2.0 ppm: methylene protons of ethylene structural units and methylene protons of hydroxyethylene structural units
[0153] 3.7 to 4.1 ppm: Methylene protons of hydroxyethylene structural units adjacent to at least one ethylene structural unit
[0154] 4.1 to 4.5 ppm: Methylene protons of hydroxyethylene structural units that are not adjacent to ethylene structural units
[0155] According to the above assignment, if the integrated value of 1.0 to 2.0 ppm is set as x, the integrated value of 3.7 to 4.1 ppm is set as y, and the integrated value of 4.1 to 4.5 ppm is set as z, the ethylene modification rate can be calculated by the following formula.
[0156] Ethylene modification rate = {(x-2y-2z) / 4} / {y+z+(x-2y-2z) / 4}
[0157] [Synthesis Examples C2, C3]
[0158] A water-soluble resin (C) was synthesized in exactly the same manner as in Synthesis Example 1 except for the conditions shown in Table 4. Table 5 shows the weight average molecular weight, ethylene modification ratio, and saponification degree of the water-soluble resin (C).
[0159] It should be noted that the obtained water-soluble resin (C) is referred to as C1, C2, C3, etc. according to the number of the synthesis example. 10 g of the obtained powder of resin C1 to C3 was taken, respectively, and put into 90 g of warm water at 85 to 95° C., and heated and stirred for 2 to 3 hours to completely dissolve.
[0160] Table 4
[0161]
[0162] Table 5
[0163]
[0164] [Synthesis Example C4]
[0165] In a glass detachable flask with a volume of 500 mL equipped with a paddle blade stirrer, a thermometer, a reflux cooling tube, and four dropping devices, 76 g of deionized water was added and the temperature was raised to the boiling reflux temperature. Then, under stirring, 166.04 g of a mixed solution of 6.76 g of an aqueous solution of 37% sodium acrylate (hereinafter referred to as SA) and 159.28 g of an aqueous solution of 80% acrylic acid (hereinafter referred to as AA), 13.3 g of an aqueous solution of 10% by mass of sodium persulfate (hereinafter referred to as NaPS), and 22.5 g of an aqueous solution of 2% by mass of hydrogen peroxide (hereinafter referred to as HP) were added dropwise for 140 minutes for a mixed solution of an SA aqueous solution and an AA aqueous solution, 160 minutes for an NaPS aqueous solution, and 140 minutes for an HP aqueous solution. After the addition was completed, the boiling reflux temperature was maintained for 30 minutes to complete the polymerization, and an aqueous solution of a light yellow, transparent, water-soluble polyacrylic acid copolymer (C4) having a solid content of 47.4% by mass was obtained. The concentration of "solid content" referred to here is a value measured by a normal pressure heating drying method (sample weight: 1.0 g, drying temperature 110°C x 2 hours) in accordance with JIS K6828-1: 2003. The weight average molecular weight was measured by gel permeation chromatography (GPC) under the above conditions and was 50,000.
[0166] [Synthesis Example C5]
[0167] In a four-necked flask equipped with a stirrer, a thermometer, a reflux cooling tube and a nitrogen inlet tube, 234.6 g of acrylamide and 960 g of ion exchange water were added, and the oxygen in the reaction system was removed by nitrogen. The temperature in the system was set to 40°C, and 0.25 g of ammonium persulfate and 0.15 g of sodium bisulfite were added as polymerization initiators under stirring. After heating to 90°C, the temperature was kept for 2 hours. After the polymerization was completed, 70 g of ion exchange water was added to obtain an aqueous solution of polyacrylamide (C5) with a solid content of 18.6% by mass. The concentration of "solid content" mentioned here refers to the value measured by the normal pressure heating drying method (sample weight: 1.0 g, drying temperature 110°C × 2 hours drying) in accordance with JIS K6828-1:2003. The weight average molecular weight was measured under the above conditions using gel permeation chromatography (GPC), and the result was 100,000.
[0168] [Synthesis Example C6]
[0169] Under the same apparatus conditions as those in Synthesis Example C5, 93.8 g of acrylamide, 960 g of ion exchange water, 93.8 g of hydroxyethyl acrylate, and 47.0 g of polyethylene glycol monomethacrylate (C3H5COO(C2H4O)4-H) were added, and oxygen in the reaction system was removed by nitrogen under the same conditions. The temperature in the system was set to 40°C, and 0.25 g of ammonium persulfate and 0.15 g of sodium bisulfite were added as polymerization initiators while stirring. After the temperature was raised to 90°C, the temperature was kept for 2 hours. After the polymerization was completed, 70 g of ion exchange water was added to obtain an aqueous solution of a polyacrylamide copolymer (C6) with a solid content of 18.6% by mass. The concentration of the "solid content" mentioned here refers to the value measured by the normal pressure heating drying method (sample weight: 1.0 g, drying temperature 110°C × 2 hours drying) in accordance with JIS K6828-1:2003. The weight average molecular weight was measured by gel permeation chromatography (GPC) under the above-mentioned conditions and was found to be 100,000.
[0170] <Preparation of ether compound (D)>
[0171] The ether compounds shown in Table 6 were prepared.
[0172] Table 6
[0173] Ether compound (D) Substance name D1 Polyvinyl alcohol D2 Polyoxyethylene lauryl ether D3 Sodium Carboxymethyl Cellulose D4 Hydroxyethyl Cellulose
[0174] <Preparation of surface treatment agent>
[0175] The surface treatment agent of each example and comparative example is prepared as follows: the water dispersion containing the composite prepared above, the water-soluble resin (C) and the ether compound (D) are mixed in the mass proportion of the solid content shown in Table 7-1, Table 7-2 and Table 7-3, and then deionized water is added so that the solid content of the obtained mixture is 100 g and the total amount is 1000 g, and the mixture is stirred. The "solid content" mentioned here refers to the value measured by the normal pressure heating drying method (sample weight: 1.0 g, drying temperature 110°C × 2 hours drying) in accordance with JIS K6828-1:2003. In addition, the solid content mass of (A), (B) and (E) in Table 7-1, Table 7-2 and Table 7-3 is calculated based on the solid content ratio of the raw materials when synthesizing the above composite. It should be noted that the composite and the water-soluble resin (C) required for the preparation of the surface treatment agent of each example and comparative example are synthesized by appropriately adding the necessary amount.
[0176]
[0177]
[0178]
[0179] <Preparation of test materials>
[0180] An aluminum test piece (A1050 manufactured by PALTEK CORPORATION, size: 70 mm×150 mm, plate thickness: 0.8 mm) was prepared.
[0181] <Formation of Surface Treatment Coating Film>
[0182] The test material was immersed in a treatment bath containing an alkali degreasing agent "Fine Cleaner 315E" (manufactured by Nippon Parkersei Co., Ltd.) adjusted to a concentration of 20 g / L and a bath temperature of 60°C for 3 minutes to remove dirt or oil attached to the surface, and then the alkali components remaining on the surface were washed with tap water.
[0183] The cleaned test material was immersed in the surface treatment agent (liquid temperature: 25°C) involved in each embodiment and comparative example for 30 seconds, and then hung in a blower dryer adjusted to 150°C for heating and drying for 6 minutes to form a surface treatment coating film on the surface of the test material. After that, it was cooled to room temperature to prepare an evaluation sample. The mass of the surface treatment coating film was 0.8 g / m 2 The solid content concentration was adjusted. Note that the evaluation samples were prepared in the number required for the following evaluation.
[0184] <Hydrophilicity Evaluation Method>
[0185] 1 μL of deionized water was dripped onto the evaluation sample prepared above, and the contact angle of the formed water drop was measured using a contact angle meter (DM-501 manufactured by Kyowa Interface Science Co., Ltd.). The contact angle of the evaluation sample cooled to room temperature after the hydrophilic treatment was taken as the initial hydrophilicity; the contact angle of the evaluation sample after immersing it in deionized water for 240 hours, drying it in an air-supplied dryer adjusted to 50°C for 1 hour and cooling it to room temperature was taken as the hydrophilicity after durability. The obtained contact angle was scored according to the criteria shown below, and a score of 3 points or more was considered to be qualified for the hydrophilicity for the purpose of the present invention. The results are shown in Tables 8-1, 8-2, and 8-3.
[0186] <Evaluation criteria for hydrophilicity>
[0187] 5 points: less than 10°
[0188] 4 points: 10° or more and less than 20°
[0189] 3 points: 20° or more and less than 30°
[0190] 2 points: 30° or more and less than 40°
[0191] 1 point: above 40°
[0192] <Corrosion resistance evaluation method>
[0193] (1)SST
[0194] According to the salt spray test method (JIS Z2371: 2015), the evaluation samples prepared above were exposed for 240 hours, and the rust area (ratio of white rust area to the total area) of the test material was evaluated by visual observation. The evaluation criteria are as follows. If the evaluation criteria value is 3 points or more, the corrosion resistance is evaluated to be good. The results are shown in Table 8-1, Table 8-2, and Table 8-3.
[0195] <Evaluation Criteria>
[0196] 5 points: White rust area is less than 10%
[0197] 4 points: White rust area is more than 10% and less than 30%
[0198] 3 points: White rust area is more than 30% and less than 50%
[0199] 2 points: White rust area is more than 50% and less than 70%
[0200] 1 point: White rust area is more than 70%
[0201] (2) SWAAT
[0202] Based on the SWAAT test (ASTM G85-A3), prepare an artificial seawater solution (ASTM D1141-98) adjusted to an aqueous solution of pH 3.0 with acetic acid. For the evaluation samples prepared above, spray (49°C × 30 minutes) with an artificial seawater solution, followed by wet exposure (49°C × 90 minutes), with a total of 120 minutes as one cycle. After 60 cycles of exposure, immerse in a 2 mass % chromic acid aqueous solution at 95°C for 10 minutes to remove white rust. The size and number of holes are evaluated by the rating method based on JIS Z2371: 2015. If the evaluation base value is 3 points or more, it is evaluated as having good pitting resistance. The results are shown in Tables 8-1, 8-2, and 8-3.
[0203] <Evaluation Criteria>
[0204] 5: RN is 9.5 or above
[0205] 4: RN is 9.3 or more and less than 9.5
[0206] 3: RN is 9 or more and less than 9.3
[0207] 2: RN is greater than 8 and less than 9
[0208] 1: RN is less than 8
[0209] <Odor Evaluation Method>
[0210] The odor of the evaluation sample prepared as above immediately after preparation is taken as the initial odor; the odor after the evaluation sample is immersed in deionized water for 240 hours, dried in a forced air dryer adjusted to 50°C for 1 hour, and cooled to room temperature is taken as the post-durable odor. The obtained odor is evaluated according to the criteria shown below. The evaluation criteria are based on the odor intensity of isovaleric acid, which is used as the standard odor of the odor component, at a predetermined concentration. When the evaluation criteria value is 3 points or more, it is regarded as the odor suppressing effect for the purpose of the present invention and is evaluated as qualified. The results are shown in Table 8-1, Table 8-2, and Table 8-3.
[0211] <Evaluation Criteria for Odor>
[0212] 5 points: No odor
[0213] 4 points: barely perceptible odor (detection threshold: isovaleric acid concentration: 0.05 μg / L)
[0214] 3 points: What kind of weak odor can be detected (cognitive threshold: isovaleric acid concentration: 0.4μg / L)
[0215] 2 points: Easily perceptible odor (detection threshold: isovaleric acid concentration: 4 μg / L)
[0216] 1 point: strong odor (detection threshold: isovaleric acid concentration: 30 μg / L)
[0217] <Dispersion stability evaluation method>
[0218] The surface treatment agents involved in each embodiment and comparative example were stored in a constant temperature bath at 40°C for 1 week, and the appearance of the liquid after storage was visually confirmed and scored as shown below. The evaluation benchmark value of 3 points or more was qualified. It should be noted that even if precipitation occurs, as long as it is used after sufficient stirring and dispersion, the other performance evaluation results are qualified, and the dispersion stability is evaluated as qualified. The results are shown in Table 8-1, Table 8-2, and Table 8-3.
[0219] <Evaluation criteria for dispersion stability>
[0220] 5 points: No precipitation
[0221] 3 points: A small amount of precipitation is produced at the bottom of the container
[0222] 1 point: A large amount of sediment was produced that completely covered the bottom of the container.
[0223] Table 8-1
[0224]
[0225] Table 8-2
[0226]
[0227] Table 8-3
[0228]
Claims
1. A surface treatment agent, wherein The surface treatment agent contains one or more selected from water-soluble inorganic oxides and salts thereof (A), one or more selected from hydrolyzates and condensates of organic alkoxysilanes (B), a water-soluble resin (C), an ether compound (D), and water and / or a water-miscible solvent. If M A 、M B 、M C and M D represents the total mass of one or more selected from water-soluble inorganic oxides and salts thereof (A), the total mass of one or more selected from hydrolyzates and condensates of organoalkoxysilanes (B), the mass of the water-soluble resin (C) and the mass of the ether compound (D), then (M A +M B ) / (M A +M B +M C +M D )=0.01~0.
7.
2. The surface treatment agent according to claim 1, wherein One or more selected from the water-soluble inorganic oxides and their salts (A) are alkaline, containing an element (M1) selected from Si, V, Zr, Mo, Ti and W and a cationic component (M2) selected from Na, K, Li and NH4, and the molar ratio (M2) / (M1) of (M2) to (M1) is 0.1 to 8.
0.
3. The surface treatment agent according to claim 1 or 2, wherein One or more selected from the water-soluble inorganic oxides and salts thereof (A) are represented by a molecular formula of the general formula Me2O·nSiO2, Me is a cationic component selected from Na, K, Li and NH4, and n is 0.5 to 8.
0.
4. The surface treatment agent according to any one of claims 1 to 3, wherein If M A 、M B represents the total mass of one or more selected from the water-soluble inorganic oxides and salts thereof (A) and the total mass of one or more selected from the hydrolyzates and condensates of the organoalkoxysilane (B), then (M A ) / (M B )=0.25~4.
0.
5. The surface treatment agent according to any one of claims 1 to 4, wherein One or more selected from the water-soluble inorganic oxides and salts thereof (A) and one or more selected from the hydrolyzates and condensates of the organoalkoxysilane (B) form a complex, wherein the median particle size of the complex measured by dynamic light scattering is 10 nm or less.
6. The surface treatment agent according to any one of claims 1 to 5, wherein The water-soluble resin (C) includes one or more selected from water-soluble resins having one or more functional groups selected from amide groups, hydroxyl groups and carboxyl groups, or water-soluble resins having amide bonds in their skeletons.
7. The surface treatment agent according to any one of claims 1 to 6, wherein If M A 、M B 、M C and M D represents the total mass of one or more selected from the water-soluble inorganic oxides and salts thereof (A), the total mass of one or more selected from the hydrolyzates and condensates of the organoalkoxysilane (B), the mass of the water-soluble resin (C), and the mass of the ether compound (D), then M D / (M A +M B +M C +M D )=0.001~0.
2.
8. A method for surface treatment of a metal material, wherein: The surface treatment method of a metal material comprises the step of bringing the surface treatment agent according to any one of claims 1 to 7 into contact with the metal material and then drying the contacted metal material.
9. A method for manufacturing a surface-treated metal material, wherein: The method for producing a surface-treated metal material comprises the step of bringing the surface treatment agent according to any one of claims 1 to 7 into contact with a metal material and then drying the contacted metal material.
10. A heat exchanger, wherein: The heat exchanger uses a surface-treated metal material obtained by the manufacturing method according to claim 9.
11. A method for surface treatment of a heat exchanger, wherein: The surface treatment method of the heat exchanger comprises the step of bringing the surface treatment agent according to any one of claims 1 to 7 into contact with the heat exchanger and then drying the contacted surface.
12. A method for manufacturing a surface treated heat exchanger, wherein: The method for producing a surface-treated heat exchanger includes a step of bringing the surface treatment agent according to any one of claims 1 to 7 into contact with a heat exchanger and then drying the contacted surface treatment agent.
13. A surface treatment heat exchanger, wherein: The surface-treated heat exchanger is obtained by the manufacturing method according to claim 12.
Citation Information
Patent Citations
Hydrophilization treatment agent for aluminum-containing metal material
CN106661420A
Hydrophilization treating composition for heat exchanger fin and method for hydrophilization treatment
JP1989249863A
Hydrophilization treatment agent for aluminum-containing metal material
JP2017179602A