Raw material for coating material for secondary battery separator, coating material for secondary battery separator, secondary battery separator, and secondary battery
By using a combination of water-soluble polymers, specific reactive surfactants and vinyl monomers in secondary battery separators, combined with inorganic particles, the problem of insufficient heat resistance, air permeability and adhesion of separator coating materials is solved. problem, significantly improving the overall performance of the diaphragm.
Patent Information
- Application Number
- CN202380024753.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-27
- Filing Date
- 2023-05-19
- Publication Date
- 2024-10-15
AI Technical Summary
Existing secondary battery separator coating materials have deficiencies in heat resistance, air permeability and adhesion, especially poor adhesion to polyolefin porous membranes, resulting in reduced performance.
Water-soluble polymers are used as raw materials for coating materials, including reactive surfactants and vinyl monomers containing acidic groups. The ratio is controlled within a specific range, and ether sulfate-type anionic reactive surfactants and amide-containing amide are added. Based on the vinyl monomer, combined with inorganic particles, a coating film is formed to improve the separator performance.
The heat resistance, air permeability and adhesion of the secondary battery separator are significantly improved, ensuring good adhesion with the porous membrane, thus improving the overall performance of the battery.
Smart Images

Figure BDA0005020177700000041 
Figure BDA0005020177700000061 
Figure BDA0005020177700000071
Abstract
Description
Technical Field
[0001] The present invention relates to a raw material for coating a secondary battery separator, a coating material for a secondary battery separator, a secondary battery separator and a secondary battery. Specifically, the present invention relates to a raw material for coating a secondary battery separator, a coating material for a secondary battery separator comprising the raw material for coating a secondary battery separator, a secondary battery separator having a coating film of the coating material for secondary battery separator, and a secondary battery having the secondary battery separator. Background Art
[0002] Conventionally, a secondary battery is provided with a separator for isolating a positive electrode from a negative electrode and allowing ions in an electrolyte solution to pass therethrough.
[0003] As such a separator, for example, a polyolefin porous film is known.
[0004] On the other hand, a coating layer may be provided on the surface of the separator from the viewpoint of imparting heat resistance. Such a coating layer contains a binder resin and inorganic particles.
[0005] In addition, examples of the binder resin include acrylic acid-based water-soluble polymers. In addition, it is known to introduce a reactive surfactant unit into an acrylic acid-based water-soluble polymer from the viewpoint of dispersibility.
[0006] As such a binder resin, for example, a water-soluble polymer including a reactive surfactant unit is proposed, wherein the reactive surfactant unit is 1 part by weight based on 101 parts by weight of the water-soluble polymer (for example, see Example 1 of Patent Document 1).
[0007] In addition, as a binder resin, a lithium ion secondary battery binder composition is proposed, which contains a water-soluble polymer including a reactive surfactant unit and 20 wt % to 70 wt % of an acid group-containing monomer unit (for example, see Patent Document 2).
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2014-222649
[0011] Patent Document 2: International Publication No. 2014 / 185381 Pamphlet Summary of the invention
[0012] Problems to be solved by the invention
[0013] However, the coating layer is required to have heat resistance, air permeability, and adhesion to the substrate (specifically, adhesion to the polyolefin porous film).
[0014] On the other hand, in Patent Document 1, since the reactive surfactant unit is small relative to the water-soluble polymer, there is a disadvantage that heat resistance, air permeability and adhesion are reduced.
[0015] In addition, in Patent Document 2, since the number of monomer units containing an acid group is large relative to the water-soluble polymer, there is a disadvantage that heat resistance, air permeability, and adhesion are reduced.
[0016] The present invention provides a raw material for a secondary battery separator coating material having excellent heat resistance, air permeability and adhesion, a secondary battery separator coating material comprising the raw material for a secondary battery separator coating material, a secondary battery separator having a coating film of the secondary battery separator coating material, and a secondary battery having the secondary battery separator.
[0017] Means for solving problems
[0018] The present invention [1] is a raw material for a coating material for a secondary battery separator, which comprises a water-soluble polymer, wherein the water-soluble polymer comprises a first structural unit derived from a reactive surfactant and a second structural unit derived from a vinyl monomer containing an acidic group, wherein the content ratio of the first structural unit in the water-soluble polymer is 3% to 30% by mass, and the content ratio of the second structural unit in the water-soluble polymer is 3% to 19% by mass.
[0019] The present invention [2] comprises the secondary battery separator coating material raw material described in [1] above, wherein the water-soluble polymer has a glass transition temperature of 150° C. or higher.
[0020] The present invention [3] includes the raw material for coating material for secondary battery separator as described in [1] or [2] above, wherein the aforementioned water-soluble polymer also contains a third structural unit derived from an amide-containing vinyl monomer, and the content ratio of the aforementioned third structural unit in the aforementioned water-soluble polymer is greater than 51% by mass and less than 94% by mass.
[0021] The present invention [4] comprises the raw material for secondary battery separator coating material according to any one of the above [1] to [3], wherein the reactive surfactant is an ether sulfate type anionic reactive surfactant.
[0022] The present invention [5] includes the raw material for secondary battery separator coating material described in [4] above, wherein the ether sulfate type anionic reactive surfactant is an ethylene oxide adduct.
[0023] The present invention [6] comprises the raw material for secondary battery separator coating material according to any one of [1] to [3] above, wherein the reactive surfactant is an ethylene oxide addition type nonionic reactive surfactant.
[0024] The present invention [7] comprises the secondary battery separator coating material raw material described in [5] or [6] above, wherein the number of moles of ethylene oxide added is 5 mol to 30 mol.
[0025] The present invention [8] includes a secondary battery separator coating material comprising the secondary battery separator coating material raw material according to any one of [1] to [7] above and inorganic particles.
[0026] The present invention [9] includes a secondary battery separator comprising: a porous membrane; and a coating film of the separator coating material according to the above [8] disposed on at least one surface of the porous membrane.
[0027] The present invention
[10] includes a secondary battery comprising a positive electrode, a negative electrode, and the secondary battery separator described in the above [9] disposed between the positive electrode and the negative electrode.
[0028] Effects of the Invention
[0029] The raw material of the secondary battery separator coating material of the present invention comprises a water-soluble polymer, wherein the water-soluble polymer comprises a first structural unit derived from a reactive surfactant and a second structural unit derived from an acidic group-containing vinyl monomer in a predetermined ratio, and thus has excellent heat resistance, air permeability and adhesion.
[0030] The secondary battery separator coating material of the present invention includes the secondary battery separator coating material raw material of the present invention, and therefore has excellent heat resistance, air permeability, and adhesion.
[0031] The secondary battery separator of the present invention includes a coating film of the secondary battery separator coating material of the present invention, and therefore has excellent heat resistance, air permeability, and adhesion.
[0032] The secondary battery of the present invention includes the secondary battery separator of the present invention, and therefore has excellent heat resistance, air permeability, and adhesion. DETAILED DESCRIPTION
[0033] <Raw materials for coating materials for secondary battery separators>
[0034] The secondary battery separator coating material raw material contains a water-soluble polymer.
[0035] The water-soluble polymer includes a first structural unit derived from a reactive surfactant and a second structural unit derived from an acidic group-containing vinyl monomer.
[0036] Such a water-soluble polymer is a polymer formed by polymerizing a water-soluble polymer raw material.
[0037] The water-soluble polymer is defined as a polymer having a residual solid content of 0.1% or less when 1 g of a temporarily dried polymer is dissolved in 100 ml of water by stirring for 24 hours and then filtered through a 300-mesh metal mesh.
[0038] The water-soluble polymer raw material comprises a reactive surfactant and a vinyl monomer containing an acidic group.
[0039] [Reactive surfactant]
[0040] The reactive surfactant is a surfactant copolymerizable with an acidic group-containing vinyl monomer. Specifically, the reactive surfactant is a surfactant having an ethylenically unsaturated group (eg, a vinyl group, a (meth)acryloyl group).
[0041] Examples of such reactive surfactants include anionic reactive surfactants and nonionic reactive surfactants.
[0042] The anionic reactive surfactant is represented by, for example, the following formula (1).
[0043] [Chemical formula 1]
[0044] Chemical formula 1
[0045]
[0046] In the above formula (1), R 1 represents a hydrogen atom or a methyl group. 1 Preferably it represents a hydrogen atom.
[0047] In the above formula (1), R 2 represents an alkylene group having 1 to 4 carbon atoms. That is, the anionic reactive surfactant represented by the above formula (1) is an alkylene oxide adduct. Examples of the alkylene group having 1 to 4 carbon atoms include methylene, ethylene, propylene and butylene. From the viewpoint of improving heat resistance, air permeability and adhesion (specifically, adhesion to a porous membrane (described later)), R 2 Preferably, it represents ethylene. That is, the anionic reactive surfactant represented by the above formula (1) is preferably an ethylene oxide adduct.
[0048] In the above formula (1), R 3represents an alkyl group. Examples of the alkyl group include a linear alkyl group and a branched alkyl group. Examples of the linear alkyl group include a linear alkyl group having 1 to 20 carbon atoms. Examples of the linear alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group (lauryl group), a tridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, and an eicosyl group.
[0049] Examples of the branched alkyl group include a branched alkyl group having 3 to 16 carbon atoms. Examples of the branched alkyl group having 3 to 16 carbon atoms include an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a 1-ethylpropyl group, a 1-methylbutyl group, a 1-methylpentyl group, a 1,1-dimethylpropyl group, a 1,1-dimethylbutyl group, a tert-hexyl group, a cyclohexyl group, a 1,1-dimethylpentyl group, a 1-methylhexyl group, a 1,1-dimethylhexyl group, a 1-methylheptyl group, a 2-methylbutyl group, a 2-ethylbutyl group, a 2,2-dimethylpropyl group, a cyclohexylmethyl group, a 2-ethylhexyl group, a 2-propylpentyl group, and a 3-methylpentyl group.
[0050] R 3 Preferably, it represents a straight-chain alkyl group. 3 More preferably, it represents a linear alkyl group having 8 to 20 carbon atoms. 3 More preferably, it represents undecyl.
[0051] In the above formula (1), R 4 represents an alkylene group. Examples of the alkylene group include linear alkylene groups and branched alkylene groups. Examples of the linear alkylene group include linear alkylene groups having 1 to 10 carbon atoms. Examples of the linear alkylene group having 1 to 10 carbon atoms include methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, nonylene, and decylene.
[0052] Examples of the branched alkylene group include alkylene groups having a carbon number of 3 or more and 10 or less. Examples of the alkylene group having a carbon number of 3 or more and 10 or less include isopropylene, isobutylene, sec-butylene, tert-butylene, isopentylene, sec-pentylene, 2-methylhexylene, and 2-ethylhexylene.
[0053] R 5 R represents an anionic hydrophilic group. Examples of anionic hydrophilic groups include carboxyl, sulfonic acid, and phosphoric acid. In addition, these functional groups may also form salts (e.g., sodium salts, potassium salts, calcium salts, magnesium salts, and ammonium salts). From the perspective of improving heat resistance, air permeability, and adhesion, R 5 Preferably, it is a salt representing a sulfonic acid group (for example, -SO3X, where X represents a salt).
[0054] That is, the anionic reactive surfactant is preferably an ether sulfate type anionic reactive surfactant. 5 More preferably, it represents -SO3NH4.
[0055] m represents 0 or 1. m preferably represents 0.
[0056] n represents the number of added moles of alkylene oxide (preferably ethylene oxide). n is, for example, 4 or more, preferably 5 or more, more preferably 10 or more, from the viewpoint of suppressing the difficulty of copolymerization of the reactive surfactant due to the decrease in solubility of the reactive surfactant in water and improving heat resistance and adhesion, and is, for example, 45 or less, preferably 40 or less, more preferably 35 or less, further preferably 30 or less, particularly preferably 25 or less, and most preferably 20 or less from the viewpoint of improving heat resistance.
[0057] Furthermore, from the viewpoint of improving heat resistance, air permeability and adhesion, the anionic reactive surfactant is preferably represented by the following formula (2).
[0058] [Chemical formula 2]
[0059] Chemical formula 2
[0060]
[0061] The anionic reactive surfactant represented by the above formula (2) is R in the above formula (1). 1 Represents a hydrogen atom, R 2 represents ethylene, R 3 represents undecyl, R 5 It represents -SO3NH4, and m represents 0, which is an anionic reactive surfactant.
[0062] In addition, commercially available products may be used as the anionic reactive surfactant. Examples of such commercially available products include ADEKA REASOAP SR series (anionic reactive surfactant represented by the above formula (2), manufactured by ADEKA Corporation).
[0063] The nonionic reactive surfactant is represented by, for example, the following formula (3).
[0064] [Chemical formula 3]
[0065] Chemical formula 3
[0066]
[0067] In the above formula (3), R 1 ~R 4 , m and n and R in the above formula (1)1 ~R 4 , m and n are synonymous.
[0068] In the above formula (3), R 1 Preferably it represents a hydrogen atom.
[0069] In the above formula (3), R 2 That is, from the viewpoint of improving heat resistance, air permeability and adhesion, the nonionic reactive surfactant is preferably an ethylene oxide adduct (ethylene oxide addition type nonionic reactive surfactant).
[0070] In the above formula (3), R 3 Preferably, it represents a straight-chain alkyl group. 3 More preferably, it represents an undecyl group. 4 Preferably, it represents a straight-chain alkylene group. 4 More preferably, it represents an ethylene group. In the above formula (3), m represents 1.
[0071] In the above formula (3), n is, for example, 4 or more, and is 5 or more, more preferably 10 or more, from the viewpoint of suppressing the difficulty of copolymerization of the reactive surfactant due to the decrease in the solubility of the reactive surfactant in water and improving the heat resistance and adhesion. In addition, n is, for example, 45 or less, preferably 40 or less, more preferably 35 or less, and from the viewpoint of improving the heat resistance, it is further preferably 30 or less, particularly preferably 25 or less, and most preferably 20 or less.
[0072] The nonionic reactive surfactant is preferably represented by the following formula (4).
[0073] [Chemical formula 4]
[0074] Chemical formula 4
[0075]
[0076] The nonionic reactive surfactant represented by the above formula (4) is R in the above formula (3). 1 Represents a hydrogen atom, R 2 represents ethylene, R 3 represents undecyl, R 4 A nonionic reactive surfactant wherein m represents 1 and ethylene is represented by a moiety.
[0077] In addition, commercially available nonionic reactive surfactants may be used. Examples of such commercially available products include ADEKA REASOAP ER series (nonionic reactive surfactants represented by the above formula (4) manufactured by ADEKA Corporation) and AQUALON KH series (nonionic reactive surfactants represented by the above formula (4) manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).
[0078] Furthermore, the reactive surfactant can be appropriately selected according to the type of the porous membrane (described later) and the type of surface treatment applied to the porous membrane (described later).
[0079] The reactive surfactant may be used alone or in combination of two or more.
[0080] The content ratio of the reactive surfactant relative to the water-soluble polymer raw material is, for example, 3% by mass or more, and from the viewpoint of further improving the adhesion, it is preferably 5% by mass or more, and is, for example, 30% by mass or less, preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 10% by mass or less, and particularly preferably 9% by mass or less.
[0081] [Acidic group-containing vinyl monomer]
[0082] Examples of the acidic group-containing vinyl monomer include a carboxyl group-containing vinyl monomer, a sulfonic acid group-containing vinyl monomer, and a phosphoric acid group-containing vinyl monomer.
[0083] The carboxyl group-containing vinyl monomer is a vinyl monomer which is copolymerizable with the reactive surfactant and contains a carboxyl group.
[0084] As the carboxyl group-containing vinyl monomer, for example, monocarboxylic acid, dicarboxylic acid, or salts thereof can be cited. As the monocarboxylic acid, for example, (meth)acrylic acid can be cited. As the dicarboxylic acid, for example, itaconic acid, maleic acid, fumaric acid, itaconic anhydride, maleic anhydride, and fumaric anhydride can be cited. It should be noted that "(meth)acrylic-" is "methacrylic-" and / or "acrylic-".
[0085] As the carboxyl group-containing vinyl monomer, preferably, monocarboxylic acid is used. As the carboxyl group-containing vinyl monomer, more preferably, (meth)acrylic acid is used. As the carboxyl group-containing vinyl monomer, further preferably, methacrylic acid is used.
[0086] The sulfonic acid group-containing vinyl monomer is a vinyl monomer which is copolymerizable with the reactive surfactant and contains a sulfonic acid group.
[0087] As the vinyl monomer containing a sulfonic acid group, for example, allyl sulfonic acid, methallyl sulfonic acid, and acrylamide tert-butyl sulfonic acid can be cited. In addition, the vinyl monomer containing a sulfonic acid group includes its salt. As the salt of the vinyl monomer containing a sulfonic acid group, for example, alkali metal salts (for example, sodium salts, potassium salts) and ammonium salts can be cited. Specifically, for example, sodium allyl sulfonate, sodium methallyl sulfonate, and ammonium methallyl sulfonate can be cited.
[0088] The vinyl monomer containing a phosphoric acid group is a vinyl monomer which is copolymerizable with a reactive surfactant and contains a phosphoric acid group.
[0089] As a vinyl monomer containing a phosphoric acid group, 2-methacryloyloxyethyl acid phosphate is mentioned, for example.
[0090] As the acidic group-containing vinyl monomer, preferably, a carboxyl group-containing vinyl monomer is used from the viewpoint of heat resistance.
[0091] The acidic group-containing vinyl monomer may be used alone or in combination of two or more.
[0092] The content ratio of the acidic group-containing vinyl monomer relative to the water-soluble polymer raw material is, for example, 3% by mass or more, preferably 5% by mass or more, and, for example, 19% by mass or less. From the viewpoint of further improving heat resistance and adhesion, it is preferably 15% by mass or less, and more preferably 10% by mass or less.
[0093] [Amide group-containing vinyl monomer]
[0094] The water-soluble polymer raw material preferably contains an amide group-containing vinyl monomer. Although described in detail later, when the water-soluble polymer raw material contains an amide group-containing vinyl monomer, the water-soluble polymer contains the third structural unit derived from the amide group-containing vinyl monomer.
[0095] The amide group-containing vinyl monomer is a vinyl monomer which can be copolymerized with a reactive surfactant and an acidic group-containing vinyl monomer and contains an amide group.
[0096] Examples of the amide group-containing vinyl monomer include methacrylamide and acrylamide.
[0097] As the amide group-containing vinyl monomer, preferably, methacrylamide is mentioned.
[0098] The amide group-containing vinyl monomer may be used alone or in combination of two or more.
[0099] The content ratio of the amide group-containing vinyl monomer relative to the water-soluble polymer raw material is, for example, 20% by mass or more, preferably 40% by mass or more, more preferably 45% by mass or more, and from the viewpoint of further improving heat resistance, air permeability and adhesion, it is further preferably 51% by mass or more, particularly preferably 60% by mass or more, and most preferably 70% by mass or more. In addition, it is, for example, 94% by mass or less, and preferably 80% by mass or less.
[0100] [Comonomer]
[0101] The water-soluble polymer raw material preferably contains a copolymerizable monomer. Although described in detail later, when the water-soluble polymer raw material contains a copolymerizable monomer, the water-soluble polymer contains the fourth structural unit derived from the copolymerizable monomer.
[0102] The copolymerizable monomer is a monomer that can copolymerize with the reactive surfactant, the vinyl monomer containing an acidic group, and the vinyl monomer containing an amide group.
[0103] Examples of copolymerizable monomers include (meth)acrylic acid alkyl esters, functional group-containing vinyl monomers (excluding acidic group-containing vinyl monomers and amide group-containing vinyl monomers), vinyl esters, aromatic vinyl monomers, N-substituted unsaturated carboxylic acid amides, heterocyclic vinyl compounds, vinylidene halide compounds, α-olefins, dienes, and crosslinkable vinyl monomers.
[0104] Examples of the alkyl (meth)acrylate include alkyl (meth)acrylates having an alkyl moiety with a carbon number of 1 to 12. Examples of the alkyl (meth)acrylates having an alkyl moiety with a carbon number of 1 to 12 include alkyl (meth)acrylates having an alkyl moiety with a carbon number of 1 to 4 and alkyl (meth)acrylates having an alkyl moiety with a carbon number of 5 to 12. Examples of the alkyl (meth)acrylates having an alkyl moiety with a carbon number of 1 to 4 include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, and tert-butyl (meth)acrylate. Examples of the alkyl (meth)acrylate having an alkyl portion having 5 to 12 carbon atoms include n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate.
[0105] As the alkyl (meth)acrylate, preferably, there are alkyl (meth)acrylates having an alkyl moiety having 1 to 4 carbon atoms.
[0106] Examples of the functional group-containing vinyl monomer (excluding acidic group-containing vinyl monomers and amide group-containing vinyl monomers) include hydroxyl group-containing vinyl monomers, amino group-containing vinyl monomers, glycidyl group-containing vinyl monomers, cyano group-containing vinyl monomers, and acetoacetoxy group-containing vinyl monomers.
[0107] As the hydroxyl-containing vinyl monomer, for example, 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate can be mentioned. As the hydroxyl-containing vinyl monomer, preferably 2-hydroxyethyl (meth)acrylate can be mentioned. As the hydroxyl-containing vinyl monomer, more preferably 2-hydroxyethyl methacrylate can be mentioned.
[0108] Examples of the amino group-containing vinyl monomer include 2-aminoethyl (meth)acrylate, 2-(N-methylamino)ethyl (meth)acrylate, and 2-(N,N-dimethylamino)ethyl (meth)acrylate.
[0109] As a glycidyl group-containing vinyl monomer, glycidyl (meth)acrylate is mentioned, for example.
[0110] Examples of the cyano group-containing vinyl monomer include (meth)acrylonitrile.
[0111] As an acetoacetoxy group-containing vinyl monomer, acetoacetoxyethyl (meth)acrylate is mentioned, for example.
[0112] Examples of the vinyl esters include vinyl acetate and vinyl propionate.
[0113] Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, and chlorostyrene.
[0114] As N-substituted unsaturated carboxylic acid amide, for example, N-methylol (meth) acrylamide is mentioned. As N-substituted unsaturated carboxylic acid amide, preferably N-methylol acrylamide is mentioned.
[0115] Examples of the heterocyclic vinyl compound include vinyl pyrrolidone.
[0116] Examples of the vinylidene halide compound include vinylidene chloride and vinylidene fluoride.
[0117] Examples of the α-olefins include ethylene and propylene.
[0118] Examples of the dienes include butadiene.
[0119] As the crosslinkable vinyl monomer, for example, a vinyl monomer containing two or more vinyl groups can be cited. As the vinyl monomer containing two or more vinyl groups, for example, methylenebis(meth)acrylamide, divinylbenzene, di(meth)acrylate containing a polyethylene glycol chain, trimethylolpropane tetraacrylate, pentaerythritol triacrylate, and pentaerythritol tetraacrylate can be cited.
[0120] As the copolymerizable monomer, preferably, a functional group-containing vinyl monomer is used. As the copolymerizable monomer, more preferably, a hydroxyl group-containing vinyl monomer is used.
[0121] The copolymerizable monomers may be used alone or in combination of two or more.
[0122] The content ratio of the copolymerizable monomer relative to the water-soluble polymer raw material is, for example, 1 mass % or more, preferably 5 mass % or more, and, for example, 60 mass % or less, preferably 40 mass % or less, more preferably 20 mass % or less, further preferably 15 mass % or less, and particularly preferably 10 mass % or less.
[0123] [Method for producing water-soluble polymer]
[0124] The water-soluble polymer can be obtained by polymerizing a water-soluble polymer raw material by a known method.
[0125] Specifically, for example, a water-soluble polymer raw material and a polymerization initiator are mixed in water, the water-soluble polymer raw material is polymerized, and then aged as necessary.
[0126] The polymerization initiator is not particularly limited, and examples thereof include water-soluble initiators, oil-soluble initiators, and redox initiators. Examples of water-soluble initiators include persulfates (e.g., ammonium persulfate, potassium persulfate), hydrogen peroxide, and organic hydrogen peroxides, and 4,4'-azobis(4-cyanovaleric acid). Examples of oil-soluble initiators include benzoyl peroxide and azobisisobutyronitrile.
[0127] As the polymerization initiator, preferably a water-soluble initiator is used, more preferably a persulfate is used, and further preferably ammonium persulfate is used.
[0128] The mixing ratio of the polymerization initiator relative to 100 parts by mass of the water-soluble polymer raw material is, for example, 0.01 parts by mass or more, preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, further preferably 0.5 parts by mass or more, and, for example, 3 parts by mass or less, preferably 1 part by mass or less.
[0129] The polymerization initiator can be used alone or in combination of two or more.
[0130] Under normal pressure, the polymerization temperature is, for example, 30° C. or higher, preferably 50° C. or higher, for example, 95° C. or lower, preferably 85° C. or lower. The polymerization time is, for example, 0.5 hour or higher, preferably 1.5 hours or higher, and for example, 20 hours or lower, preferably 10 hours or lower.
[0131] The aging time is, for example, 0.5 hours or more, preferably 1.5 hours or more, and, for example, 8 hours or less, preferably 6 hours or less.
[0132] In addition, in the above-mentioned polymerization, from the viewpoint of achieving improved manufacturing stability, known additives such as pH adjusters, metal ion sealants (for example, ethylenediaminetetraacetic acid and its salts), molecular weight regulators (chain transfer agents) (for example, thiols, low molecular weight halogen compounds) can be added in appropriate proportions.
[0133] In addition, before or after the above-mentioned polymerization, a neutralizing agent such as ammonia may be added to adjust the pH to a range of 5 to 11.
[0134] Thereby, the polymer as the water-soluble polymer raw material is obtained as an aqueous solution containing the water-soluble polymer.
[0135] The solid content concentration of the aqueous solution containing the water-soluble polymer is, for example, 10 mass % or more, and for example, 50 mass % or less.
[0136] As described above, the water-soluble polymer is formed by polymerizing a water-soluble polymer raw material containing a reactive surfactant and an acidic group-containing vinyl monomer.
[0137] Therefore, the water-soluble polymer includes a first structural unit derived from the reactive surfactant and a second structural unit derived from the acidic group-containing vinyl monomer.
[0138] The content ratio of the first structural unit in the water-soluble polymer is 3% by mass or more, and from the viewpoint of further improving the adhesion, it is preferably 5% by mass or more, and is 30% by mass or less, preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 10% by mass or less, and particularly preferably 9% by mass or less.
[0139] When the content ratio of the first structural unit is not less than the above lower limit, heat resistance, air permeability, and adhesion can be improved.
[0140] On the other hand, when the content ratio of the first structural unit is less than the above lower limit, heat resistance, air permeability, and adhesion are reduced.
[0141] Moreover, when the content ratio of the first structural unit is equal to or less than the above upper limit, heat resistance, air permeability, and adhesion can be improved.
[0142] On the other hand, when the content ratio of the first structural unit exceeds the above upper limit, heat resistance, air permeability, and adhesion decrease.
[0143] It should be noted that the content ratio of the first structural unit can be calculated from the amount of the reactive surfactant charged. That is, the content ratio of the first structural unit is synonymous with the content ratio of the reactive surfactant relative to the water-soluble polymer raw material.
[0144] In addition, the content ratio of the second structural unit in the water-soluble polymer is 3 mass % or more, preferably 5 mass % or more, and is 19 mass % or less. From the viewpoint of further improving heat resistance and adhesion, it is preferably 15 mass % or less, and more preferably 10 mass % or less.
[0145] When the content ratio of the second structural unit is not less than the above lower limit, heat resistance, air permeability, and adhesion can be improved.
[0146] On the other hand, when the content ratio of the second structural unit is less than the above lower limit, heat resistance, air permeability and adhesion are reduced.
[0147] Moreover, when the content ratio of the second structural unit is equal to or less than the above upper limit, heat resistance, air permeability, and adhesion can be improved.
[0148] On the other hand, when the content ratio of the second structural unit exceeds the above upper limit, heat resistance, air permeability, and adhesion are reduced.
[0149] It should be noted that the content ratio of the second structural unit can be calculated from the input amount of the acidic group-containing vinyl monomer. That is, the content ratio of the second structural unit is synonymous with the content ratio of the acidic group-containing vinyl monomer relative to the water-soluble polymer raw material.
[0150] In addition, in the water-soluble polymer, the mass ratio of the first structural unit to the second structural unit (first structural unit / second structural unit) is, for example, greater than 0.1, preferably greater than 0.2, more preferably greater than 0.3, and, for example, less than 15.0, preferably less than 10.0, more preferably less than 7.0, and further preferably less than 5.0.
[0151] When the mass ratio is not less than the lower limit and not more than the upper limit, heat resistance, air permeability, and adhesion can be improved.
[0152] When the water-soluble polymer raw material contains an amide group-containing vinyl monomer, the water-soluble polymer contains a third structural unit derived from the amide group-containing vinyl monomer.
[0153] The content ratio of the third structural unit in the water-soluble polymer is, for example, 20 mass % or more, preferably 40 mass % or more, more preferably 45 mass % or more, and from the viewpoint of further improving heat resistance, air permeability and adhesion, it is further preferably 51 mass % or more, particularly preferably 60 mass % or more, most preferably 70 mass % or more, and, for example, 94 mass % or less, preferably 80 mass % or less.
[0154] When the content ratio of the third structural unit is not less than the above lower limit, heat resistance, air permeability, and adhesion can be improved.
[0155] Moreover, when the content ratio of the third structural unit is equal to or less than the above upper limit, heat resistance, air permeability, and adhesion can be improved.
[0156] It should be noted that the content ratio of the third structural unit can be calculated from the amount of the amide group-containing vinyl monomer charged. That is, the content ratio of the third structural unit is synonymous with the content ratio of the amide group-containing vinyl monomer relative to the water-soluble polymer raw material.
[0157] When the water-soluble polymer raw material contains a copolymerizable monomer, the water-soluble polymer contains the fourth structural unit derived from the copolymerizable monomer.
[0158] The content ratio of the fourth structural unit in the water-soluble polymer is, for example, 1% by mass or more, preferably 5% by mass or more, and, for example, 60% by mass or less, preferably 40% by mass or less, more preferably 20% by mass or less, further preferably 15% by mass or less, and particularly preferably 10% by mass or less.
[0159] When the content ratio of the fourth structural unit is not less than the above lower limit, heat resistance, air permeability, and adhesion can be improved.
[0160] Moreover, when the content ratio of the fourth structural unit is equal to or less than the above upper limit, heat resistance, air permeability, and adhesion can be improved.
[0161] The content of the fourth structural unit can be calculated from the amount of the copolymerizable monomer charged. That is, the content of the fourth structural unit is synonymous with the content of the copolymerizable monomer relative to the water-soluble polymer raw material.
[0162] The water-soluble polymer preferably includes the first structural unit and the second structural unit, and the third structural unit and the fourth structural unit.
[0163] The glass transition temperature of the water-soluble polymer is, for example, 120°C or higher, preferably 150°C or higher, more preferably 180°C or higher, further preferably 200°C or higher, particularly preferably 210°C or higher, most preferably 220°C or higher, and, for example, 300°C or lower.
[0164] The glass transition temperature can be measured, for example, using Discrete DSC2500 manufactured by TA Instruments.
[0165] In the above manner, a coating material raw material for a secondary battery separator containing a water-soluble polymer is obtained.
[0166] Moreover, the secondary battery separator coating material raw material comprises a water-soluble polymer, and the water-soluble polymer comprises a first structural unit from a reactive surfactant and a second structural unit from a vinyl monomer containing an acidic group in a prescribed ratio. Therefore, heat resistance, air permeability and adhesion are excellent. Moreover, such a secondary battery separator coating material raw material can be used appropriately in the manufacture of a secondary battery separator coating material.
[0167] <Coating material for secondary battery separator>
[0168] The secondary battery separator coating material includes a secondary battery separator coating material raw material and inorganic particles.
[0169] As inorganic particles, for example, oxides, nitrides, carbides, sulfates, hydroxides and potassium titanate can be mentioned. As oxides, for example, aluminum oxide, silicon dioxide, titanium dioxide, zirconium oxide, magnesium oxide, cerium dioxide, yttrium oxide, zinc oxide and iron oxide can be mentioned. As nitrides, for example, silicon nitride, titanium nitride and boron nitride can be mentioned. As carbides, for example, silicon carbide and calcium carbonate can be mentioned. As sulfates, for example, magnesium sulfate and aluminum sulfate can be mentioned. As hydroxides, for example, aluminum hydroxide and diaspore can be mentioned. As silicates, for example, talc, kaolinite, dickite, pearl clay, halloysite, pyrophyllite, montmorillonite, sericite, mica, magnesia chlorite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, silica sand and glass can be mentioned. As inorganic particles, hydroxides can be preferably mentioned. As inorganic particles, diaspore can be more preferably mentioned.
[0170] The average particle diameter of the inorganic particles is, for example, 0.1 μm or more, preferably 0.5 μm or more, and, for example, 5 μm or less, preferably 1 μm or less.
[0171] The average particle size of the inorganic particles can be determined by preparing a particle size distribution curve using a laser diffraction / scattering particle size distribution measuring apparatus and calculating a particle size corresponding to 50% by mass.
[0172] The inorganic particles may be used alone or in combination of two or more.
[0173] The mixing ratio of the inorganic particles relative to 100 parts by mass of the secondary battery separator coating material raw material is, for example, 1000 parts by mass or more, for example, 10000 parts by mass or less, and preferably 5000 parts by mass or less.
[0174] In order to produce the secondary battery separator coating material, first, inorganic particles and, if necessary, a dispersant are mixed in water to prepare an inorganic particle dispersion. When a dispersant is mixed, the secondary battery separator coating material contains the dispersant.
[0175] Examples of the dispersant include ammonium polycarboxylate and sodium polycarboxylate. Preferably, ammonium polycarboxylate is used as the dispersant.
[0176] The mixing ratio of the dispersant relative to 100 parts by mass of the inorganic particles is, for example, 0.5 parts by mass or more, preferably 1 part by mass or more, and, for example, 10 parts by mass or less, preferably 5 parts by mass or less.
[0177] The dispersants may be used alone or in combination of two or more.
[0178] Next, the secondary battery separator coating material raw material is mixed into the inorganic particle dispersion and stirred.
[0179] The stirring method is not particularly limited, and examples thereof include ball mills, bead mills, planetary ball mills, vibration ball mills, sand mills, colloid mills, attritors, roll mills, high-speed impeller dispersion, dispersers, homogenizers, high-speed impact mills, ultrasonic dispersion, and stirring blades.
[0180] In addition, the secondary battery separator coating material may contain additives such as a hydrophilic resin, a wetting agent, a defoaming agent, and a pH adjuster at appropriate ratios as needed. That is, the secondary battery separator coating material contains additives as needed.
[0181] These additives may be used alone or in combination of two or more.
[0182] In addition, the details will be described later, but in the secondary battery separator coating material, even without a wetting agent, the heat resistance and adhesion can be improved. Therefore, it is preferred not to mix a wetting agent in the secondary battery separator coating material. In other words, the secondary battery separator coating material preferably does not substantially contain a wetting agent. The so-called secondary battery separator coating material does not substantially contain a wetting agent, which means that: relative to the secondary battery separator coating material, the wetting agent content ratio is, for example, 0.1% by mass or less, preferably 0.01% by mass or less, and more preferably 0.001% by mass or less.
[0183] Thus, a secondary battery separator coating material (aqueous dispersion of a secondary battery separator coating material) was obtained.
[0184] The solid content concentration of the aqueous dispersion of the secondary battery separator coating material is, for example, 10 mass % or more, preferably 20 mass % or more, more preferably 30 mass % or more, and, for example, 50 mass % or less.
[0185] The coating material for secondary battery separators includes the above-mentioned raw material for coating material for secondary battery separators. Therefore, the coating material has excellent heat resistance, air permeability and adhesion. Moreover, such a coating material for secondary battery separators can be used appropriately in the manufacture of secondary battery separators.
[0186] <Secondary battery separator>
[0187] The secondary battery separator includes a porous film and a coating film of a secondary battery separator coating material disposed on at least one surface of the porous film.
[0188] [Porous membrane]
[0189] As the porous film, for example, polyolefin porous film and aromatic polyamide porous film can be mentioned. As the polyolefin porous film, for example, polyethylene porous film and polypropylene porous film can be mentioned. As the porous film, preferably polyolefin porous film can be mentioned. The porous film can be surface treated as needed. As the surface treatment, for example, corona treatment and plasma treatment can be mentioned.
[0190] The thickness of the porous film is, for example, 1 μm or more, preferably 5 μm or more, and, for example, 40 μm or less, preferably 20 μm or less.
[0191] [Coating film]
[0192] The coating film is a heat-resistant layer for imparting heat resistance to the porous film and is formed of a coating material for a secondary battery separator.
[0193] The thickness of the coating film is, for example, 1 μm or more, preferably 3 μm or more, and, for example, 10 μm or less, preferably 8 μm or less.
[0194] [Method for producing secondary battery separator]
[0195] The method for producing a secondary battery separator comprises the following steps: a first step of preparing a porous membrane; and a second step of applying a separator coating material on at least one surface of the porous membrane.
[0196] (1st step)
[0197] In the first step, a porous membrane is prepared.
[0198] (Second step)
[0199] In the second step, a coating material for a secondary battery separator (aqueous dispersion of a coating material for a secondary battery separator) is applied to at least one surface of the porous membrane and then dried as necessary to obtain a coating film.
[0200] There are no particular restrictions on the coating method, and examples thereof include gravure coating, small-diameter gravure coating, reverse roll coating, transfer roll coating, kiss coating, dip coating, micro gravure coating, knife coating, air knife coating, blade coating, rod coating, extrusion coating, cast coating, die coating, screen printing, and spray coating.
[0201] The drying temperature is, for example, 40° C. or higher, and, for example, 80° C. or lower.
[0202] In this way, a secondary battery separator is produced which includes a porous membrane and a coating film of the secondary battery separator coating material disposed on at least one surface of the porous membrane.
[0203] In the above description, the coating film of the secondary battery separator coating material is disposed on at least one surface of the porous membrane, but the coating film may be disposed on both surfaces of the porous membrane.
[0204] The secondary battery separator has a coating film of the above-mentioned secondary battery separator coating material. Therefore, it has excellent heat resistance, air permeability and adhesion. Moreover, such a secondary battery separator can be used appropriately in the manufacture of secondary batteries.
[0205] <Secondary Battery>
[0206] The secondary battery includes a positive electrode, a negative electrode, the secondary battery separator disposed between the positive electrode and the negative electrode, and an electrolyte impregnated in the positive electrode, the negative electrode, and the secondary battery separator.
[0207] As the positive electrode, for example, a known electrode including a positive electrode current collector and a positive electrode active material stacked on the positive electrode current collector can be used.
[0208] Examples of the positive electrode current collector include conductive materials such as aluminum, titanium, stainless steel, nickel, calcined carbon, conductive polymers, and conductive glass.
[0209] The positive electrode active material is not particularly limited, and examples thereof include known positive electrode active materials such as lithium-containing transition metal oxides, lithium-containing phosphates, and lithium-containing sulfates.
[0210] These positive electrode active materials may be used alone or in combination of two or more.
[0211] As the negative electrode, for example, a known electrode including a negative electrode current collector and a negative electrode active material stacked on the negative electrode current collector can be used.
[0212] Examples of the negative electrode current collector include conductive materials such as copper and nickel.
[0213] The negative electrode active material is not particularly limited, and examples thereof include carbon active materials. Examples of the carbon active material include graphite, soft carbon, and hard carbon.
[0214] These negative electrode active materials may be used alone or in combination of two or more.
[0215] When a lithium ion battery is used as the secondary battery, the electrolyte may be, for example, a solution in which a lithium salt is dissolved in a carbonate compound such as ethylene carbonate (EC), propylene carbonate (PC), or ethyl methyl carbonate (EMC).
[0216] To manufacture a secondary battery, for example, a separator of the secondary battery is sandwiched between a positive electrode and a negative electrode, these are housed in a battery case (battery cell), and an electrolyte is injected into the battery case.
[0217] In this way, a secondary battery can be obtained.
[0218] Since the secondary battery described above includes the secondary battery separator described above, it is excellent in heat resistance, air permeability, and adhesion.
[0219] <Effects>
[0220] The raw material of the coating material for secondary battery separators contains a water-soluble polymer containing a first structural unit derived from a reactive surfactant and a second structural unit derived from an acidic group-containing vinyl monomer at a predetermined ratio, and thus has excellent heat resistance, air permeability and adhesion.
[0221] Specifically, from the viewpoint of improving heat resistance and adhesion, it has been studied to add a wetting agent to the secondary battery separator coating material containing the secondary battery separator coating material raw material.
[0222] As a result, the secondary battery separator coating material is fixed to the surface of the porous membrane to a greater extent, and the heat resistance and adhesion can be improved. However, when a wetting agent is added, the free wetting agent penetrates into the porous membrane, and the air permeability decreases.
[0223] On the other hand, the raw material of the secondary battery separator coating material contains a water-soluble polymer containing a first structural unit derived from a reactive surfactant and a second structural unit derived from an acidic group-containing vinyl monomer at a predetermined ratio.
[0224] Thus, even without adding a wetting agent to the secondary battery separator coating material, heat resistance and adhesion can be improved, and since no wetting agent is added, the above-mentioned reduction in air permeability due to free wetting agent can be suppressed, resulting in improved air permeability.
[0225] The secondary battery separator coating material includes the secondary battery separator coating material raw material, and therefore has excellent heat resistance, air permeability, and adhesion.
[0226] The secondary battery separator includes a coating film of the secondary battery separator coating material, and therefore has excellent heat resistance, air permeability, and adhesion.
[0227] The secondary battery includes the secondary battery separator, and therefore has excellent heat resistance, air permeability, and adhesion.
[0228] Example
[0229] Next, the present invention is described based on examples and comparative examples, but the present invention is not limited to the following examples. It should be noted that, unless otherwise specified, "parts" and "%" are based on mass. In addition, the specific numerical values of the mixing ratio (containing ratio), physical property values, parameters, etc. used in the following description can be replaced by the upper limit value (numerical value defined in the form of "below", "less than") or the lower limit value (numerical value defined in the form of "above", "greater than") of the corresponding mixing ratio (containing ratio), physical property values, parameters, etc. recorded in the above-mentioned "specific implementation method".
[0230] <Details of ingredients>
[0231] The details of the active ingredients used in the following Examples and Comparative Examples are shown below.
[0232] SR-10: ADEKA REASOAP SR-10, a compound represented by the above formula (2) (n=10), number of moles of ethylene oxide added: 10, manufactured by ADEKA Corporation
[0233] SR-20: ADEKA REASOAP SR-20, a compound represented by the above formula (2) (n=20), number of moles of ethylene oxide added: 20, manufactured by ADEKA Corporation
[0234] ER-10: ADEKA REASOAP ER-10, a compound represented by the above formula (4) (n=10), number of moles of ethylene oxide added: 10, manufactured by ADEKA Corporation
[0235] ER-20: ADEKA REASOAP ER-20, a compound represented by the above formula (4) (n=20), number of moles of ethylene oxide added: 20, manufactured by ADEKA Corporation
[0236] ER-30: ADEKA REASOAP ER-30, a compound represented by the above formula (4) (n=30), number of moles of ethylene oxide added: 30, manufactured by ADEKA Corporation
[0237] ER-40: ADEKA REASOAP ER-40, a compound represented by the above formula (4) (n=40), number of moles of ethylene oxide added: 40, manufactured by ADEKA Corporation
[0238] KH-05: AQUALON KH-05: The compound represented by the above formula (4) (n=5), number of moles of ethylene oxide added: 5, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.
[0239] Mam: Methacrylic acid
[0240] Mac: Methacrylamide
[0241] HEMA: 2-Hydroxyethyl Methacrylate
[0242] <Manufacturing of coating material raw material for secondary battery separator, coating material for secondary battery separator, and secondary battery separator>
[0243] Example 1
[0244] [Manufacturing of coating material raw materials for secondary battery separators]
[0245] 392.0 parts by mass of distilled water were added to a detachable flask with a stirrer and a reflux condenser, and after replacing with nitrogen, the temperature was raised to 80°C. Next, after adding 0.6 parts by mass of ammonium persulfate, SR-10, Mac, Mam and HEMA were dissolved in water in a manner such that the first to fourth structural units were in the proportions described in Table 1, partially neutralized with aqueous ammonia, and added continuously for 3 hours, and further maintained for 3 hours to complete the polymerization. An appropriate amount of water was added to obtain an aqueous solution of a water-soluble polymer having a solid content of 15.0% by mass. The pH of the water-soluble polymer is 6.0. Thus, a raw material for a coating material for a secondary battery separator containing a water-soluble polymer was manufactured.
[0246] [Manufacturing of coating material for secondary battery separator]
[0247] An inorganic particle dispersion was prepared by uniformly dispersing 100 parts by mass of diaspore (Boehmite Grade C06, particle size: 0.7 μm, manufactured by Daemyung Chemical Co., Ltd.) as inorganic particles and 3.0 parts by mass (calculated as solid content) of an aqueous solution of ammonium polycarboxylate (SN Dispersant 5468, manufactured by SAN NOPCO Co., Ltd.) as a dispersant in 110 parts by mass of water.
[0248] Next, the secondary battery separator coating material raw material was added to the inorganic particle dispersion in an amount of 5 parts by mass in terms of solid content, water was added in an amount of 40% by mass of solid content, and the mixture was stirred for 15 minutes. Thus, a secondary battery separator coating material was produced.
[0249] [Manufacturing of secondary battery separators]
[0250] (1st step)
[0251] As a porous membrane, a polyolefin resin porous membrane was prepared. Specifically, as a polyolefin resin porous membrane, a product number SW509C+ (film thickness 9.6 μm, porosity 40.6%, air permeability 158 g / 100 ml, surface density 5.5 g / m 2 , Changzhou Xingyuan New Energy Materials Co., Ltd.).
[0252] Next, the surface of the polyolefin resin porous membrane was cut into A4 size.
[0253] (Second step)
[0254] Using a wire rod, a coating material for a secondary battery separator (aqueous dispersion of a coating material for a secondary battery separator) is applied to the surface (one side) of a polyolefin resin porous membrane. Then, it is dried at 50°C. Thus, a coating film (thickness of 5 μm) is formed on the surface (one side) of the polyolefin resin porous membrane. Thus, a secondary battery separator is manufactured.
[0255] Examples 2 to 20 and Comparative Examples 1 to 8
[0256] A secondary battery separator coating material raw material, a secondary battery separator coating material, and a secondary battery separator were produced by the same procedure as in Example 1. However, the formulation of each component was changed so that the first to fourth structural units were in the ratios described in Tables 1 to 3.
[0257] <Evaluation>
[0258] [Glass transition temperature of water-soluble polymer]
[0259] The glass transition temperature of the water-soluble polymer of each embodiment and each comparative example was measured. Specifically, the glass transition temperature was measured using Discovery DSC2500 manufactured by TA Instruments under measurement conditions 1: RT / 300°C (held for 1 minute) / -90°C (held for 3 minutes); heating rate 50°C / min, cooling rate 10°C / min, 2nd heating rate 10°C / min, nitrogen atmosphere. The results are shown in Tables 1 to 3.
[0260] [Heat resistance]
[0261] The secondary battery separator of each embodiment and each comparative example was cut into 5 cm × 5 cm and used as a test piece. After the test piece was placed in an oven at 150°C × 1 hour, the length of each side was measured and the thermal shrinkage was calculated. The heat resistance was evaluated according to the following criteria. The results are shown in Tables 1 to 3.
[0262] (Benchmark)
[0263] ◎: Thermal shrinkage is less than 5%.
[0264] ○: The heat shrinkage rate is 5% or more and less than 20%.
[0265] △: The heat shrinkage rate is 20% or more and less than 50%.
[0266] ×: The heat shrinkage rate is 50% or more.
[0267] [Breathability]
[0268] For the secondary battery separators of each embodiment and each comparative example, the air permeability was measured according to JIS-P-8117 using a Wangyan air permeability smoothness tester manufactured by Asahi Seiko Co., Ltd. The smaller the air permeability, the better the air permeability can be evaluated. The air permeability was evaluated according to the following criteria. The results are shown in Tables 1 to 3.
[0269] (Benchmark)
[0270] ◎: Air permeability is less than 210s / 100ml.
[0271] ○: Air permeability is 210 s / 100 ml or more and less than 250 s / 100 ml.
[0272] ×: Air permeability is 250s / 100ml or more.
[0273] [Adhesion]
[0274] The adhesion of the secondary battery separators of each example and each comparative example was measured. Specifically, the coating film in the secondary battery separator was rubbed with a rubber. The adhesion was evaluated according to the following criteria. The results are shown in Tables 1 to 3.
[0275] (Benchmark)
[0276] ◎: No peeling even after rubbing 5 times with a load of 400 g. ○: Peeling after rubbing less than 5 times with a load of 400 g. ×: Peeling after rubbing with a load of 100 g.
[0277] [Table 1]
[0278]
[0279] [Table 2]
[0280]
[0281] [Table 3]
[0282]
[0283] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, which is merely an illustration and is not to be construed as limiting. Modifications of the present invention that are obvious to those skilled in the art are also included in the appended claims.
[0284] Industrial Applicability
[0285] The secondary battery separator coating material raw material, secondary battery separator coating material, and secondary battery separator of the present invention can be suitably used, for example, in the production of secondary batteries. The secondary battery of the present invention can be suitably used, for example, in various devices and automobiles.
Claims
1. A coating material raw material for a secondary battery separator, comprising a water-soluble polymer, The water-soluble polymer comprises a first structural unit derived from a reactive surfactant and a second structural unit derived from an acidic group-containing vinyl monomer. The content ratio of the first structural unit in the water-soluble polymer is 3% by mass or more and 30% by mass or less, The content ratio of the second structural unit in the water-soluble polymer is 3 mass % or more and 19 mass % or less.
2. The raw material for coating the secondary battery separator according to claim 1, wherein The water-soluble polymer has a glass transition temperature of 150° C. or higher.
3. The raw material for coating the secondary battery separator according to claim 1, wherein The water-soluble polymer further comprises a third structural unit derived from an amide-containing vinyl monomer, The content ratio of the third structural unit in the water-soluble polymer is 51 mass % or more and 94 mass % or less.
4. The raw material for coating the secondary battery separator according to claim 1, wherein The reactive surfactant is an anionic reactive surfactant of ether sulfate type.
5. The raw material for coating the secondary battery separator according to claim 4, wherein The ether sulfate type anionic reactive surfactant is an ethylene oxide adduct.
6. The raw material for coating the secondary battery separator according to claim 1, wherein The reactive surfactant is an ethylene oxide addition type nonionic reactive surfactant.
7. The raw material for coating the secondary battery separator according to claim 5, wherein: The number of moles of ethylene oxide added is 5 mol or more and 30 mol or less. 8 . A coating material for a secondary battery separator, comprising the raw material for a coating material for a secondary battery separator according to claim 1 and inorganic particles.
9. A secondary battery separator having: a porous membrane; and A coating film of the separator coating material according to claim 8 disposed on at least one surface of the porous membrane. 10 . A secondary battery comprising a positive electrode, a negative electrode, and the secondary battery separator according to claim 9 disposed between the positive electrode and the negative electrode.