A desulfurizing agent and preparation method thereof

By combining materials such as epoxy nanosilica, triazine phenolic resin, carbon nanotube modified silane and activated carbon, the desulfurization agent is prepared to form a mesh structure, which solves the problem of insufficient desulfurization efficiency and accuracy in the prior art, and realizes the Highly efficient adsorption and removal of hydrogen sulfide gas.

CN118788314BActive Publication Date: 2024-11-26DONGYING HAIXIN HEATING SUPPLY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411274492.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-26
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The desulfurization efficiency, accuracy and penetration sulfur capacity of the existing iron-zinc-based lignin activated carbon desulfurizer are insufficient, making it difficult to effectively remove hydrogen sulfide gas.

Method used

Desulfurization agent is prepared by combining epoxy nanosilica, triazine phenolic resin, carbon nanotube modified silane, activated carbon and N-methyldiethanolamine. The network structure is formed through condensation, quaternization, esterification and other reactions to improve the Adsorption site and absorption effect.

Benefits of technology

It significantly improves the desulfurization efficiency and accuracy, increases the penetration of sulfur capacity, and achieves more efficient adsorption and removal of hydrogen sulfide gas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the technical field of chemical desulfurization, and discloses a desulfurizer and a preparation method thereof. The present invention is to add epoxy nano-silicon dioxide, triazine-based phenolic resin, carbon nanotube modified silane, activated carbon, and N-methyldiethanolamine into a stirrer, and stir to obtain a desulfurizer. During stirring, the epoxy group in the epoxy nano-silicon dioxide will undergo a ring-opening reaction with the phenolic hydroxyl group in the triazine-based phenolic resin and the amino group in the carbon nanotube modified silane, forming a tight cross-linked network with each other, providing more adsorption sites, and hydrogen sulfide gas can be better adsorbed through the mesh structure. The triazine group, epoxy nano-silicon dioxide, carbon nanotube structure, and phenolic resin in the desulfurizer themselves have a good adsorption effect on hydrogen sulfide gas; at the same time, the triazine-based phenolic resin contains a large amount of quaternary ammonium salt, which has a good absorption effect on hydrogen sulfide gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical desulfurization, in particular to a desulfurizing agent and a preparation method thereof. Background Art

[0002] Hydrogen sulfide is a poisonous and harmful acidic gas with a rotten egg smell. The formation pathway of hydrogen sulfide is very extensive, mainly present in natural gas, coke oven gas and petroleum cracking gas. If it is discharged into the air, it will pollute the environment, thereby endangering human health. For example, patent CN106925229B provides a kind of iron-zinc-based composite lignin activated carbon desulfurizer, and the preparation method is: lignin activated carbon is dissolved in zinc salt solution, iron salt solution and surfactant reaction are added, and then a certain concentration of alkaline solution is used to titrate the mixed ultrasonic reaction to obtain an iron-zinc-based lignin activated carbon desulfurizer, and the desulfurization effect is good, but its desulfurization efficiency and sulfur capacity need to be improved. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies in the prior art, the present invention provides a desulfurizer and a preparation method thereof, which have good desulfurization efficiency, and also high desulfurization accuracy and penetration sulfur capacity.

[0005] (II) Technical solution

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a desulfurizer and a preparation method thereof, comprising the following components by weight: 4-10 parts by weight of epoxy nano-silica, 5-8 parts by weight of triazine-based phenolic resin, 4-7 parts by weight of carbon nanotube-modified silane, 15-30 parts by weight of activated carbon, and 7-10 parts by weight of N-methyldiethanolamine.

[0007] Preferably, the preparation method of the triazine-based phenolic resin is:

[0008] (1) Add 2,4,6-tris(4-formylphenyl)-1,3,5-triazine and lysine to isopropanol solvent, stir and mix, heat to 35-50°C, react for 6-12h, then continue to add tris(dimethylamino)silane and chloroplatinic acid catalyst, react at 70-90°C for 8-14h, filter and wash after reaction to obtain triazine silane;

[0009] (2) adding 5-12 parts by weight of triazine silane and 7-10 parts by weight of chloroacetic acid to N,N-dimethylformamide solvent, stirring to dissolve, stirring for 10-15 minutes, heating to 75-90° C. to carry out quaternization reaction, and after the reaction, distilling under reduced pressure, washing and drying to obtain quaternary ammonium salt modified silane;

[0010] (3) Adding 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol and quaternary ammonium salt-modified silane to N,N-dimethylformamide solvent, and then adding p-toluenesulfonic acid catalyst thereto to carry out esterification reaction, reacting at 110-125° C. for 7-12 hours, and then rotary distilling, washing, and drying to obtain a phenol-based intermediate;

[0011] (4) 80-90 parts by weight of phenol, 14-18 parts by weight of phenol intermediate and 40-60 parts by weight of formaldehyde aqueous solution are mixed uniformly, 1-2 parts by weight of sodium hydroxide are added at 65-75° C., the mixture is stirred uniformly for reaction, water is removed by vacuum distillation, the mixture is washed with petroleum ether and dried to obtain a triazine-based phenolic resin.

[0012] Preferably, the mass ratio of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, lysine, tris(dimethylamino)silane and chloroplatinic acid catalyst in (1) is 1:2.4-3.8:2.6-3.2:0.01-0.03.

[0013] Preferably, the reaction time in (2) is 5-9 hours.

[0014] Preferably, in (3), the mass ratio of 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol, quaternary ammonium salt-modified silane, and p-toluenesulfonic acid catalyst is 1.2-1.4:1:0.02-0.03.

[0015] Preferably, the reaction time in (4) is 2-6 hours.

[0016] Preferably, the preparation method of the carbon nanotube-modified silane is:

[0017] S1. 5-12 parts by weight of a quaternary ammonium salt-modified silane and 11-16 parts by weight of thionyl chloride are added to a dimethylformamide solvent, heated to 100-110 ° C and refluxed for 6-9h, then cooled to room temperature and distilled under reduced pressure to obtain an acyl chloride silane;

[0018] S2. Add 2-5 parts by weight of carbon nanotubes to concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1 for acidification; then add the acidified carbon nanotubes to N,N-dimethylacetamide, ultrasonically disperse, continue to add 7-9 parts by weight of acyl chloride silane and 0.4-0.6 parts by weight of pyridine catalyst, react at 60-80°C for 9-11 hours, centrifuge after the reaction, wash with acetone, and dry to obtain carbon nanotube-modified silane.

[0019] Preferably, the preparation method of the desulfurizer is: adding epoxy nano-silica, triazine-based phenolic resin, carbon nanotube-modified silane, activated carbon, and N-methyldiethanolamine into a stirrer, stirring for 5-8 minutes, and obtaining the desulfurizer.

[0020] 3. Beneficial technical effects

[0021] The invention prepares the desulfurizing agent by adding epoxy nano silicon dioxide, triazine-based phenolic resin, carbon nanotube modified silane, activated carbon and N-methyldiethanolamine into a stirrer and stirring.

[0022] The aldehyde group in 2,4,6-tris(4-formylphenyl)-1,3,5-triazine and the amino group in lysine are subjected to condensation reaction to generate a double bond, and then the product is further subjected to addition reaction with tris(dimethylamino)silane to introduce a carboxyl group, thereby obtaining triazine-based silane; the tertiary amine group in the triazine-based silane and the chlorine in chloroacetic acid are subjected to quaternization reaction to generate a quaternary ammonium salt to obtain a quaternary ammonium salt-modified silane; the phenolic hydroxyl group in 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol and the carboxyl group in the quaternary ammonium salt-modified silane are subjected to esterification reaction to obtain a phenol-based intermediate; phenol, the phenol intermediate and a formaldehyde aqueous solution are reacted to obtain a triazine-based phenolic resin; the quaternary ammonium salt-modified silane is reacted with thionyl chloride to obtain an acyl chloride-based silane, and then the quaternary ammonium salt-modified silane is further reacted with the acidified carbon nanotube to obtain a carbon nanotube-modified silane.

[0023] During the stirring process, the epoxy groups in the epoxy nano-silica will undergo a ring-opening reaction with the phenolic hydroxyl groups in the triazine-based phenolic resin and the amino groups in the carbon nanotube-modified silane, increasing their compatibility with each other, forming a tight cross-linked network, providing more adsorption sites, and reducing the agglomeration of nano-silica and carbon nanotubes. Hydrogen sulfide gas can be better adsorbed through the network structure. The triazine groups, epoxy nano-silica, carbon nanotube structure, and phenolic resin in the desulfurizer have a good adsorption effect on hydrogen sulfide gas; at the same time, the triazine-based phenolic resin contains a large amount of quaternary ammonium salt, and the tertiary amine group in the triazine-based silane and the chlorine in the chloroacetic acid undergo a quaternization reaction to generate a quaternary ammonium salt, which increases the degree of substitution of the quaternary ammonium salt and makes it better for the absorption of hydrogen sulfide gas. DETAILED DESCRIPTION

[0024] The preparation method of epoxy nano-silica refers to "Silane coupling agent KH-560 modified nano-silica" in "Chemical World" Volume 3, Issue 8, August 2011; weigh a certain amount of nano-SiO2, add 20mL of toluene, and use KQ-300E ultrasonic cleaner (300W) for ultrasonic dispersion at room temperature for 30 minutes to obtain a uniform suspension, then add silane coupling agent KH-560 and continue ultrasonic dispersion for 3-4 minutes, transfer to a 100mL four-necked flask equipped with a reflux condenser and a power-enhanced electric stirrer, and stir to react in an oil bath at a set temperature. The slurry after the reaction is centrifuged at a speed of 12000r / min at room temperature using a CT15RT desktop high-speed refrigerated centrifuge to obtain epoxy nano-silica. Example 1

[0025] (1) Add 2,4,6-tris(4-formylphenyl)-1,3,5-triazine and lysine to isopropanol solvent, stir and mix, heat to 35°C, react for 6 hours, then continue to add tris(dimethylamino)silane and chloroplatinic acid catalyst, wherein the mass ratio of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, lysine, tris(dimethylamino)silane, and chloroplatinic acid catalyst is 1:2.4:2.6:0.01, react at 70°C for 8 hours, filter and wash after completion to obtain triazine silane;

[0026] (2) Add 5 parts by weight of triazine silane and 7 parts by weight of chloroacetic acid into N,N-dimethylformamide solvent, stir to dissolve, stir for 10 minutes, heat to 75°C for quaternization reaction, wherein the reaction time is 5 hours, and after the reaction, vacuum distillation, washing and drying to obtain quaternary ammonium salt modified silane;

[0027] (3) adding 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol and quaternary ammonium salt-modified silane to N,N-dimethylformamide solvent, and then adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol, quaternary ammonium salt-modified silane, and p-toluenesulfonic acid catalyst is 1.2:1:0.02, and performing esterification reaction at 110° C. for 7 hours, and then performing rotary distillation, washing, and drying to obtain a phenol-based intermediate;

[0028] (4) 80 parts by weight of phenol, 14 parts by weight of phenol intermediate, and 40 parts by weight of formaldehyde aqueous solution were mixed uniformly, 1 part by weight of sodium hydroxide was added at 65° C., and the mixture was stirred uniformly for reaction, wherein the reaction time was 2 hours, water was removed by distillation under reduced pressure, and the mixture was washed with petroleum ether and dried to obtain a triazine-based phenolic resin;

[0029] (5) adding 5 parts by weight of quaternary ammonium salt-modified silane and 11 parts by weight of thionyl chloride into dimethylformamide solvent, heating to 100° C. and reflux reaction for 6 h, cooling to room temperature, and distilling under reduced pressure to obtain acyl chloride silane;

[0030] (6) adding 2 parts by weight of carbon nanotubes to concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1 for acidification; then adding the acidified carbon nanotubes to N,N-dimethylacetamide, ultrasonically dispersing, and continuing to add 7 parts by weight of acyl chloride silane and 0.4 parts by weight of pyridine catalyst thereto, reacting at 60° C. for 9 hours, centrifuging after the reaction, washing with acetone, and drying to obtain carbon nanotube-modified silane;

[0031] (7) Add 4 parts by weight of epoxy nano-silica, 5 parts by weight of triazine-based phenolic resin, 4 parts by weight of carbon nanotube-modified silane, 15 parts by weight of activated carbon, and 7-10 parts by weight of N-methyldiethanolamine into a stirrer and stir for 5 minutes to obtain a desulfurizer. Example 2

[0032] (1) Add 2,4,6-tris(4-formylphenyl)-1,3,5-triazine and lysine to isopropanol solvent, stir and mix, heat to 50°C, react for 12 hours, then continue to add tris(dimethylamino)silane and chloroplatinic acid catalyst, wherein the mass ratio of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, lysine, tris(dimethylamino)silane, and chloroplatinic acid catalyst is 1:3.8:3.2:0.03, react at 90°C for 14 hours, filter and wash after reaction to obtain triazine silane;

[0033] (2) adding 12 parts by weight of triazine silane and 10 parts by weight of chloroacetic acid into N,N-dimethylformamide solvent, stirring to dissolve, stirring for 15 minutes, heating to 90° C. to carry out quaternization reaction, wherein the reaction time is 9 hours, and after the reaction, vacuum distillation, washing and drying to obtain quaternary ammonium salt modified silane;

[0034] (3) adding 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol and quaternary ammonium salt-modified silane to N,N-dimethylformamide solvent, and then adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol, quaternary ammonium salt-modified silane, and p-toluenesulfonic acid catalyst is 1.4:1:0.03, and carrying out esterification reaction at 125°C for 12h, and then rotary distilling, washing, and drying to obtain a phenol-based intermediate;

[0035] (4) 90 parts by weight of phenol, 18 parts by weight of phenol intermediate, and 60 parts by weight of formaldehyde aqueous solution were mixed uniformly, 2 parts by weight of sodium hydroxide were added at 75° C., and the mixture was stirred uniformly for reaction, wherein the reaction time was 6 hours, water was removed by distillation under reduced pressure, and the mixture was washed with petroleum ether and dried to obtain a triazine-based phenolic resin;

[0036] (5) adding 12 parts by weight of quaternary ammonium salt-modified silane and 16 parts by weight of thionyl chloride into dimethylformamide solvent, heating to 110° C. and reflux reaction for 9 hours, cooling to room temperature, and distilling under reduced pressure to obtain acyl chloride silane;

[0037] (6) adding 5 parts by weight of carbon nanotubes to concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1 for acidification; then adding the acidified carbon nanotubes to N,N-dimethylacetamide, ultrasonically dispersing, and continuing to add 9 parts by weight of acyl chloride silane and 0.6 parts by weight of pyridine catalyst thereto, reacting at 80° C. for 11 hours, centrifuging after the reaction, washing with acetone, and drying to obtain carbon nanotube-modified silane;

[0038] (7) 10 parts by weight of epoxy nano-silica, 8 parts by weight of triazine-based phenolic resin, 7 parts by weight of carbon nanotube-modified silane, 30 parts by weight of activated carbon, and 10 parts by weight of N-methyldiethanolamine were added into a stirrer and stirred for 8 minutes to obtain a desulfurizer. Example 3

[0039] (1) Add 2,4,6-tris(4-formylphenyl)-1,3,5-triazine and lysine to isopropanol solvent, stir and mix, heat to 42°C, react for 9 hours, then continue to add tris(dimethylamino)silane and chloroplatinic acid catalyst, wherein the mass ratio of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, lysine, tris(dimethylamino)silane, and chloroplatinic acid catalyst is 1:3.1:2.4:0.02, react at 60°C for 12 hours, filter and wash after completion to obtain triazine silane;

[0040] (2) adding 8 parts by weight of triazine silane and 8 parts by weight of chloroacetic acid into N,N-dimethylformamide solvent, stirring to dissolve, stirring for 12 minutes, heating to 82° C. to carry out quaternization reaction, wherein the reaction time is 7 hours, and after the reaction, vacuum distillation, washing and drying to obtain quaternary ammonium salt modified silane;

[0041] (3) adding 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol and quaternary ammonium salt-modified silane to N,N-dimethylformamide solvent, and then adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol, quaternary ammonium salt-modified silane, and p-toluenesulfonic acid catalyst is 1.3:1:0.025, and performing esterification reaction at 117° C. for 9 hours, and then performing rotary distillation, washing, and drying to obtain a phenol-based intermediate;

[0042] (4) 85 parts by weight of phenol, 16 parts by weight of phenol intermediate, and 50 parts by weight of formaldehyde aqueous solution were mixed uniformly, 1.5 parts by weight of sodium hydroxide were added at 70° C., and the mixture was stirred uniformly for reaction, wherein the reaction time was 3 hours, water was removed by distillation under reduced pressure, and the mixture was washed with petroleum ether and dried to obtain a triazine-based phenolic resin;

[0043] (5) adding 8 parts by weight of quaternary ammonium salt-modified silane and 13 parts by weight of thionyl chloride into dimethylformamide solvent, heating to 105° C. and reflux reaction for 7 h, cooling to room temperature, and distilling under reduced pressure to obtain acyl chloride silane;

[0044] (6) adding 3 parts by weight of carbon nanotubes to concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1 for acidification; then adding the acidified carbon nanotubes to N,N-dimethylacetamide, ultrasonically dispersing, and continuously adding 8 parts by weight of acyl chloride silane and 0.5 parts by weight of pyridine catalyst thereto, reacting at 70° C. for 10 hours, centrifuging after the reaction, washing with acetone, and drying to obtain carbon nanotube-modified silane;

[0045] (7) Add 7 parts by weight of epoxy nano-silica, 6 parts by weight of triazine-based phenolic resin, 5 parts by weight of carbon nanotube-modified silane, 22 parts by weight of activated carbon, and 8 parts by weight of N-methyldiethanolamine into a stirrer and stir for 6 minutes to obtain a desulfurizer.

[0046] Comparative Example 1

[0047] 7 parts by weight of epoxy nano-silica, 5 parts by weight of carbon nanotube-modified silane, 22 parts by weight of activated carbon, and 8 parts by weight of N-methyldiethanolamine were added into a stirrer and stirred for 6 minutes to obtain a desulfurizing agent.

[0048] Comparative Example 2

[0049] 7 parts by weight of epoxy nano-silica, 6 parts by weight of triazine-based phenolic resin, 22 parts by weight of activated carbon, and 8 parts by weight of N-methyldiethanolamine were added into a stirrer and stirred for 6 minutes to obtain a desulfurizer.

[0050] The test conditions for the desulfurization performance evaluation are: the diameter of the reaction tube is 10mm, the sample filling volume is 2ml, the reaction bed height: diameter ratio = 5:1, the temperature is 390℃, the atmospheric pressure, and the reaction gas is hydrogen sulfide standard gas (concentration 4%, the balance gas is hydrogen). The test steps are as follows: First, the hydrogen sulfide standard gas is passed through the reactor bed at a low space velocity (400h-1). After 1 hour, the space velocity is increased to 2500h-1. When 5% of sulfur is absorbed on the desulfurizer, the hydrogen sulfide concentration at the reactor outlet is detected with a hydrogen sulfide detection tube. When the desulfurizer penetrates (the hydrogen sulfide concentration at the reactor outlet is ≥200ppm), the feed is stopped, and the breakthrough sulfur capacity is calculated based on the volume of gas introduced, the odor concentration and the sample weight. The sulfur capacity test is carried out in accordance with HG / T 2513, and the test results are shown in Table 1.

[0051]

[0052] As can be seen from Table 1, compared with Comparative Example 1-2, Example 1-3 of the present invention has a larger breakthrough sulfur capacity, a higher desulfurization accuracy, a larger sulfur capacity, and a better desulfurization effect.

[0053] The desulfurization rate test was carried out with reference to ASTM D4810-88 (1999) "Standard Method for Determination of Hydrogen Sulfide Content in Natural Gas by Colorimetric Detector Tube Method". The test results are shown in Table 2.

[0054] Table 2: Desulfurization rate test.

[0055]

[0056] It can be seen from Table 2 that Examples 1-3 of the present invention have better desulfurization efficiency than Comparative Examples 1-2.

[0057] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A desulfurizing agent, characterized in that: The invention comprises the following components by weight: 4-10 parts by weight of epoxy nano-silica, 5-8 parts by weight of triazine-based phenolic resin, 4-7 parts by weight of carbon nanotube-modified silane, 15-30 parts by weight of activated carbon, and 7-10 parts by weight of N-methyldiethanolamine; The preparation method of the triazine-based phenolic resin is: (1) Add 2,4,6-tris(4-formylphenyl)-1,3,5-triazine and lysine to isopropanol solvent, stir and mix, heat to 35-50°C, react for 6-12h, then continue to add tris(dimethylamino)silane and chloroplatinic acid catalyst, react at 70-90°C for 8-14h, filter and wash after reaction to obtain triazine silane; (2) adding 5-12 parts by weight of triazine silane and 7-10 parts by weight of chloroacetic acid to N,N-dimethylformamide solvent, stirring to dissolve, stirring for 10-15 minutes, heating to 75-90° C. to carry out quaternization reaction, and after the reaction, distilling under reduced pressure, washing and drying to obtain quaternary ammonium salt modified silane; (3) Adding 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol and quaternary ammonium salt-modified silane to N,N-dimethylformamide solvent, and then adding p-toluenesulfonic acid catalyst thereto to carry out esterification reaction, reacting at 110-125° C. for 7-12 hours, and then rotary distilling, washing, and drying to obtain a phenol-based intermediate; (4) 80-90 parts by weight of phenol, 14-18 parts by weight of phenol intermediate, and 40-60 parts by weight of formaldehyde aqueous solution are mixed uniformly, 1-2 parts by weight of sodium hydroxide are added at 65-75° C., the mixture is stirred uniformly for reaction, water is removed by distillation under reduced pressure, the mixture is washed with petroleum ether, and the mixture is dried to obtain a triazine-based phenolic resin; The preparation method of the carbon nanotube-modified silane is as follows: S1. 5-12 parts by weight of a quaternary ammonium salt-modified silane and 11-16 parts by weight of thionyl chloride are added to a dimethylformamide solvent, heated to 100-110 ° C and refluxed for 6-9h, then cooled to room temperature and distilled under reduced pressure to obtain an acyl chloride silane; S2. Add 2-5 parts by weight of carbon nanotubes to concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1 for acidification; then add the acidified carbon nanotubes to N,N-dimethylacetamide, ultrasonically disperse, continue to add 7-9 parts by weight of acyl chloride silane and 0.4-0.6 parts by weight of pyridine catalyst, react at 60-80°C for 9-11 hours, centrifuge after the reaction, wash with acetone, and dry to obtain carbon nanotube-modified silane.

2. The desulfurizing agent according to claim 1, characterized in that The mass ratio of 2,4,6-tris(4-formylphenyl)-1,3,5-triazine, lysine, tris(dimethylamino)silane and chloroplatinic acid catalyst in (1) is 1:2.4-3.8:2.6-3.2:0.01-0.

03.

3. The desulfurizing agent according to claim 1, characterized in that The reaction time in (2) is 5-9h.

4. The desulfurizing agent according to claim 1, characterized in that The mass ratio of 2-(3-hydroxy-1-phenylpropyl)-4-methylphenol, quaternary ammonium salt-modified silane and p-toluenesulfonic acid catalyst in (3) is 1.2-1.4:1:0.02-0.

03.

5. The desulfurizing agent according to claim 1, characterized in that: The reaction time in (4) is 2-6 hours.

6. A method for preparing a desulfurizing agent according to any one of claims 1 to 5, characterized in that: The preparation method of the desulfurizer is as follows: adding epoxy nano-silica, triazine-based phenolic resin, carbon nanotube-modified silane, activated carbon and N-methyldiethanolamine into a stirrer, stirring for 5-8 minutes, and obtaining the desulfurizer.

Citation Information

Patent Citations

  • A zinc-iron composite lignin activated carbon desulfurizer and its preparation method

    CN106925229B

  • Pottery clay desulfurizer and preparation method thereof

    CN103736357A

  • Coating for capturing sulfides

    CN107771204A

  • Adsorbent for simultaneously removing heavy metals and VOCs in waste gas, and preparation method thereof

    CN112138637A

  • Solid amine adsorbent for removing trace hydrogen sulfide, and preparation method thereof

    CN113231037A