Indoor thermal insulation board and preparation method thereof

Through sepiolite adsorption of polyvinyl alcohol, inorganic flame retardant deposition and silica aerogel coating technology, combined with zinc hydroxystannate and cross-linking of ethylene-vinyl acetate copolymer, the problem of flammable and flammable polystyrene insulation boards is solved. The problem of thermal insulation performance degradation at high temperatures is achieved by achieving better thermal insulation, flame retardant and mechanical properties.

CN118791773AInactive Publication Date: 2024-10-18HENAN SHOUXIN BIOLOGICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411082718.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polystyrene insulation boards are flammable and the organic binders are susceptible to thermal decomposition at high temperatures, resulting in reduced thermal insulation performance and low aerogel strength and poor mechanical properties.

Method used

Sepiolite is used to absorb polyvinyl alcohol and deposit inorganic flame retardants, silica aerogel is coated with modified glass wool felt, and zinc hydroxystannate is cross-linked with ethylene-vinyl acetate copolymer to form a three-dimensional network structure to enhance the material's Thermal insulation, flame retardant and mechanical properties.

Benefits of technology

It improves the thermal insulation, flame retardant and mechanical properties of the polystyrene insulation board, enhances the structural integrity and impact resistance of the material, reduces the thermal conductivity, and avoids the thermal decomposition of the organic binder and the shrinkage of the aerogel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004984235820000101
    Figure BDA0004984235820000101
  • Figure BDA0004984235820000111
    Figure BDA0004984235820000111
Patent Text Reader

Abstract

The invention discloses an indoor thermal insulation board and a preparation method thereof, and belongs to the technical field of building thermal insulation board materials.The preparation method comprises the following steps that modified glass wool felt is soaked in silicon dioxide sol, and modified glass wool felt loaded aerogel is obtained through sealing and aging; the preparation method comprises the following steps: modifying polystyrene particles by adopting a composite material, mixing with modified glass wool felt loaded aerogel and a compatilizer, uniformly stirring, extruding in a double-screw extruder, drawing, cooling and pelletizing to obtain polystyrene board particles, mixing the polystyrene board particles with a foaming agent, adding into a plastic extruding machine, and carrying out extrusion molding to obtain the thermal insulation board. Polyvinyl alcohol permeates into a space channel in the sepiolite, so that the situation that the heat insulation and heat preservation performance is reduced due to the fact that organic binder components of the glass wool felt are easily heated and decomposed at high temperature is avoided, and the good heat insulation and heat preservation performance is achieved; the zinc hydroxystannate and the ethylene-vinyl acetate copolymer are crosslinked to form a three-dimensional network structure, so that the thermal stability of the copolymer is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building thermal insulation board materials, in particular to an indoor thermal insulation board and a preparation method thereof. Background Art

[0002] Insulation board is a rigid foam plastic board made of polystyrene resin as raw material, other raw and auxiliary materials and polymers, which is heated and mixed while injecting catalysts, and then extruded and pressed into shape. It has moisture-proof and waterproof properties, and can reduce the thickness of the building's external protective structure, thereby increasing the indoor usable area. Insulation boards are divided into organic insulation boards and inorganic insulation boards. Organic insulation boards include polystyrene boards, extruded boards, etc., which have good thermal insulation effects, light weight and low cost. Polystyrene insulation boards are lightweight materials formed by foamed polystyrene resins. They have many advantages, including excellent thermal insulation, chemical resistance and easy processing. Therefore, polystyrene foam insulation boards have been widely used in construction, packaging materials and other fields.

[0003] Polystyrene insulation boards are easy to deform, and they expand and contract in hot and cold environments for a long time, causing the boards to crack, increase water absorption, and deteriorate the insulation effect. In addition, polystyrene insulation boards are flammable materials and can easily cause fires. By adding aerogel, the thermal insulation performance of polystyrene resin boards can be effectively improved, but aerogels are prone to shrinkage and cracking, resulting in low strength and poor mechanical properties of aerogel materials, which affects the thermal insulation of aerogels. Using glass wool felt as the skeleton of aerogel can effectively improve the mechanical properties of aerogels, but the organic binder components in the glass wool felt are easily decomposed by heat at high temperatures, resulting in a decrease in the thermal insulation performance of the glass wool felt. Summary of the invention

[0004] The purpose of the present invention is to provide an indoor thermal insulation board and a preparation method thereof: sepiolite absorbs polyvinyl alcohol, and the polyvinyl alcohol penetrates into the internal space channel of the sepiolite to prevent the organic binder component of the glass wool felt from being easily decomposed by heat at high temperature, resulting in a decrease in thermal insulation performance; inorganic flame retardant is deposited on the surface of the glass wool felt loaded with sepiolite to prevent the glass wool felt from contacting each other, thereby increasing the specific surface area of ​​the glass wool felt, improving the thermal insulation performance, and improving the flame retardant performance of the glass wool felt; silica aerogel is coated on the modified glass wool felt, and the modified glass wool felt serves as the support and skeleton of the aerogel, thereby improving the strength and force of the aerogel The thermal insulation and mechanical properties of the aerogel are enhanced by mixing zinc hydroxystannate with ethylene-vinyl acetate copolymer emulsion. The zinc hydroxystannate and the ester group in the ethylene-vinyl acetate copolymer are cross-linked through hydrogen bonds to form a three-dimensional network structure, which improves the thermal stability of the copolymer. At the same time, it can also greatly increase the viscosity of the copolymer and increase the bonding force between the polystyrene particles and the inorganic material. The composite material modifies the polystyrene particles to improve the toughness and impact resistance of the particles themselves. The zinc hydroxystannate has good smoke suppression performance and can suppress the toxic smoke released when the polystyrene insulation board is burned.

[0005] Technical problems to be solved by the present invention: polystyrene insulation board is a flammable material and can easily cause fire; by adding aerogel, the thermal insulation performance of polystyrene resin board can be effectively improved, but aerogel is prone to shrinkage and cracking, resulting in low strength and poor mechanical properties of aerogel material, affecting the thermal insulation of aerogel; using glass wool felt as the skeleton of aerogel can effectively improve the mechanical properties of aerogel, but the organic binder component in the glass wool felt is easily thermally decomposed at high temperature, resulting in a decrease in the thermal insulation performance of the glass wool felt.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a flexible high temperature resistant silicone protective film comprises the following steps:

[0008] S1. Using sepiolite to adsorb polyvinyl alcohol, coating it on the surface of glass wool, curing and molding to obtain a sepiolite-loaded glass wool felt, and depositing an inorganic flame retardant on the surface of the sepiolite-loaded glass wool felt to obtain a modified glass wool felt;

[0009] Furthermore, after the sepiolite absorbs polyvinyl alcohol, it is coated on the surface of glass wool and solidified to form: 0.5 g of sepiolite is added to 50 mL of deionized water, stirred evenly, 2 mL of 0.1 mol / L hydrochloric acid is added to adjust the pH to 4.6, stirred at a speed of 12000 rpm for 30 min to obtain a suspension, 3 g of polyvinyl alcohol is added to 30 mL of deionized water, stirred at 90° C. for 4 h, added to the suspension, stirred for 2 h to obtain a mixture, the mixture is evenly sprayed on the glass wool, solidified to obtain a glass wool felt loaded with sepiolite;

[0010] The crystal structure of sepiolite is composed of continuous tetrahedral silicon-oxygen sheets. Each silicon-oxygen tetrahedron shares two corner vertices and is connected with three adjacent tetrahedrons to form an open channel. Under acidic conditions, the pores are more stable, and polyvinyl alcohol can penetrate into the internal space channels of the sepiolite, thereby preventing the organic binder polyvinyl alcohol component of the glass wool felt from being easily decomposed by heat at high temperatures, resulting in a decrease in thermal insulation performance. In addition, the hydroxyl groups on the polyvinyl alcohol molecular chain can be combined with the hydroxyl groups on the surface of the sepiolite through hydrogen bonds, thereby increasing the mechanical properties of the sepiolite itself and preventing the sepiolite from being brittle.

[0011] It should also be noted that the sepiolite in the mixture has excellent adhesion and can adhere to the surface of the glass wool.

[0012] Furthermore, the surface area of ​​sepiolite is as high as 900m 2 / g, pore diameter is 50-100nm.

[0013] Furthermore, the ratio of sepiolite to hydrochloric acid is (0.3-0.7) g:(1-3) mL.

[0014] Furthermore, the curing temperature is 200° C. and the curing time is 15 min.

[0015] Furthermore, the inorganic flame retardant is deposited on the surface of the loaded sepiolite glass wool felt as follows:

[0016] Add 0.45 g of inorganic flame retardant to 60 mL of ethanol solution and stir evenly to obtain a dispersion. Spray the dispersion on the surface of the loaded sepiolite glass wool felt and dry it in an oven at 80° C. for 30 min to evaporate the organic solvent to obtain a modified glass wool felt.

[0017] Among them, the inorganic flame retardant dispersion is evenly sprayed onto the surface of the loaded sepiolite glass wool felt, and is treated at 80°C to evaporate the ethanol solvent, so that the inorganic flame retardant is evenly deposited on the surface of the glass wool felt. The inorganic flame retardant reduces the pore size of the glass wool felt, increases the porosity, and thereby increases the thermal insulation performance.

[0018] Furthermore, the inorganic flame retardant is one of aluminum hydroxide, magnesium hydroxide and red phosphorus, and the particle size is 30-40nm.

[0019] S2. The modified glass wool felt is impregnated into the silica sol, and after sealing and aging, a loaded modified glass wool felt aerogel is obtained;

[0020] Further, the silica sol step is specifically as follows: 5g of tetraethyl orthosilicate is added to 25mL of ethanol and 75mL of deionized water, stirred for 30min, 3mL of hydrochloric acid with a concentration of 0.5mol / L is added, the temperature is raised to 50°C, stirred for 30min, and then allowed to stand for 24h to fully hydrolyze the tetraethyl orthosilicate, 20mL of deionized water and 1mL of 60% ammonia water are added, and stirred for 30min to obtain a silica sol;

[0021] In the mixed solution of ethanol and deionized water, ethyl orthosilicate is hydrolyzed to form a network sol connected by Si-O-Si bonds.

[0022] Furthermore, the modified glass wool felt is impregnated into the silica sol and subjected to sealing aging as follows:

[0023] Add 0.4 g of modified glass wool felt to 15 g of silica sol, then add 15 g of silica sol until it just covers the glass wool felt, seal and age for 24 h, add 20 mL of deionized water and 80 mL of ethanol for aging for 12 h, then add 2 g of tetraethyl orthosilicate and 20 mL of ethanol for secondary aging for 12 h, add a mixed solution of isopropanol and n-hexane to replace the organic solvent, and then add a mixed solution of 2 g of trimethylchlorosilane and 10 mL of n-hexane for surface modification. When the gel becomes transparent, wash it 3 times with n-hexane and dry it in an oven at 60 °C for 24 h to obtain a loaded modified glass wool felt aerogel.

[0024] Among them, the sol-gel method is adopted, and the modified glass wool felt is used as the support and skeleton of the aerogel, so that the silica aerogel is coated with the modified glass wool felt, which improves the strength and mechanical properties of the aerogel, reduces the direct contact between the modified glass wool felts, increases the contact area, and reduces the thermal conductivity; the silicon hydroxyl structure contained in the surface of the aerogel formed can be combined with trimethylchlorosilane through chemical bonds, so that trimethylchlorosilane can be grafted on the surface of the aerogel, thereby improving the hydrophobicity of the aerogel and avoiding the shortcomings of increased thermal conductivity and deterioration of mechanical properties caused by water and moisture absorption of the porous structure.

[0025] Furthermore, the usage ratio of modified glass wool felt and silica sol is (0.2-0.6) g:(28-32) g.

[0026] Furthermore, the porosity of the loaded modified glass wool felt aerogel is 92% and the pore size is 10-20 nm.

[0027] S3. Mixing zinc hydroxystannate with ethylene-vinyl acetate copolymer emulsion to obtain a composite material, and using the composite material to modify polystyrene particles to obtain modified polystyrene particles.

[0028] Furthermore, the zinc hydroxystannate is mixed with the ethylene-vinyl acetate copolymer emulsion by adding 0.5 g of zinc hydroxystannate to 40 g of the ethylene-vinyl acetate copolymer emulsion, stirring evenly, placing in a mixer, heating to 100° C., mixing for 30 minutes, cooling to room temperature, and taking out to obtain a composite material.

[0029] Among them, the hydroxyl groups contained on the surface of zinc hydroxystannate can be combined with the ester groups in ethylene-vinyl acetate copolymer through hydrogen bonds to form cross-linking. The introduction of the cross-linking structure enables the ethylene-vinyl acetate copolymer to form a three-dimensional network structure, thereby improving the thermal stability of the polymer. Zinc hydroxystannate has good smoke suppression properties and can suppress the smoke released when the polystyrene insulation board burns.

[0030] Furthermore, the dosage ratio of zinc hydroxystannate to ethylene-vinyl acetate copolymer emulsion is (0.3-0.7) g:(38-42) g.

[0031] Furthermore, the viscosity of the ethylene-vinyl acetate copolymer emulsion is 4000-5000 mPa·s.

[0032] Furthermore, the composite material was used to modify the polystyrene particles as follows: 3 g of the composite material was added to 50 mL of ethanol, stirred until the composite material was completely dissolved, 30 mL of deionized water was added for dilution, 1.8 g of polystyrene particles were added, stirred evenly, filtered, and dried in an oven at 80 °C for 10 min to obtain modified polystyrene particles.

[0033] Among them, in the organic solvent ethanol, the composite material solution has good adhesion after dilution, and can adhere to the surface of polystyrene particles, so that the composite material is coated on the polystyrene particles, improving the toughness and impact resistance of the particles themselves. The composite material emulsion has good adhesion and contains hydrophilic groups, which can better bond with the loaded modified glass wool felt aerogel.

[0034] Furthermore, the usage ratio of the composite material, ethanol and deionized water is (2-4) g:(45-55) mL:(25-35) mL.

[0035] Furthermore, the polystyrene particles are expanded polystyrene particles with a particle size of 2-5 mm and a bulk density of 10-12 kg / m 3 .

[0036] S4. The modified polystyrene particles, loaded modified glass wool felt aerogel and compatibilizer are mixed, stirred evenly, and extruded in a twin-screw extruder. After drawing, cooling and pelletizing, polystyrene board particles are obtained. The polystyrene board particles are mixed with a foaming agent, added to an extruder for extrusion molding, and obtained as a thermal insulation board.

[0037] Furthermore, the compatibilizer is prepared by mixing polycaprolactone and calcium stearate in a mass ratio of (3-5) g:(1.5-1.5) g, and the foaming agent is butane.

[0038] Furthermore, the temperature of the twin-screw extruder zone 1 is 230° C., the temperature of the zone 2 is 235° C., the temperature of the zone 3 is 237° C., the temperature of the zone 4 is 240° C., the temperature of the zone 5 is 245° C., and the main engine speed is 500 rpm.

[0039] Furthermore, compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) In the technical scheme of the present invention, sepiolite has good heat shielding performance, and polyvinyl alcohol is infiltrated into the internal space channel of the sepiolite, so that the organic binder component of the glass wool felt is easily decomposed by heat at high temperature, resulting in a decrease in thermal insulation performance, and the glass wool felt has good thermal insulation performance. The polymer adsorbed by the sepiolite is used as a reinforcing material to improve the mechanical properties of the sepiolite and avoid the brittleness of the sepiolite. The surface of the glass wool felt loaded with sepiolite contains a large number of hydroxyl structures, which can be combined with the inorganic flame retardant through chemical bonds to achieve the deposition of flame retardant on the surface of the glass wool felt, avoid mutual contact between the glass wool felts, increase the specific surface area of ​​the glass wool felt, and improve the thermal insulation performance. The inorganic material has good flame retardant properties, which improves the flame retardant properties of the glass wool felt, thereby improving the flame retardant properties of the organic thermal insulation board.

[0041] (2) In the technical solution of the present invention, silica aerogel is used to coat modified glass wool felt, and the modified glass wool felt serves as the support and skeleton of the aerogel, thereby improving the strength and mechanical properties of the aerogel, making the aerogel composite material have better structural integrity, thereby enhancing the thermal insulation and mechanical properties of the aerogel, and reducing the direct contact between the modified glass wool felts, increasing the contact area, and reducing the thermal conductivity, so that the loaded modified glass wool felt aerogel has a lower thermal conductivity and better thermal insulation performance. In terms of reducing the thermal conductivity, it has a synergistic effect with the inorganic combustion aid deposited on the surface of the glass wool felt.

[0042] (3) In the technical scheme of the present invention, the hydroxyl groups contained on the surface of zinc hydroxystannate can be combined with the ester groups in the ethylene-vinyl acetate copolymer through hydrogen bonds to form cross-linking, so that the zinc hydroxystannate is uniformly dispersed in the ethylene-vinyl acetate copolymer. The introduction of the cross-linking structure enables the ethylene-vinyl acetate copolymer to form a three-dimensional network structure, thereby improving the thermal stability of the copolymer. At the same time, it can also greatly increase the viscosity of the copolymer, thereby increasing the bonding force between the polystyrene particles and the inorganic material. The composite material is used to coat the polystyrene particles to improve the toughness and impact resistance of the particles themselves, and the zinc hydroxystannate has good smoke suppression performance, which can suppress the toxic smoke released when the polystyrene insulation board is burned. In addition, the hydrophilic groups contained in the composite material can achieve better bonding with the loaded modified glass wool felt aerogel, thereby enhancing the thermal insulation and flame retardant properties. DETAILED DESCRIPTION

[0043] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] Example 1

[0045] The modified glass wool felt is prepared by the following steps:

[0046] A1. Add 0.5g of sepiolite to 50mL of deionized water, stir evenly, add 2mL of 0.1mol / L hydrochloric acid to adjust the pH to 4.6, stir at 12000rpm for 30min to obtain a suspension, add 3g of polyvinyl alcohol to 30mL of deionized water, stir at 90°C for 4h, add to the suspension, stir for 2h to obtain a mixture, spray the mixture evenly on the glass wool, solidify at 200°C for 15min to obtain a glass wool felt loaded with sepiolite;

[0047] A2. Add 0.45 g of inorganic flame retardant to 60 mL of ethanol solution and stir evenly to obtain a dispersion. Spray the dispersion on the surface of the loaded sepiolite glass wool felt and dry it in an oven at 80°C for 30 min to evaporate the organic solvent to obtain a modified glass wool felt.

[0048] Comparative Example 1

[0049] The difference between this comparative example and Example 1 is that no sepiolite is added.

[0050] Add 3 g of polyvinyl alcohol into 30 mL of deionized water, spray evenly on the glass wool, and solidify at 200° C. for 15 min to obtain glass wool felt.

[0051] Comparative Example 2

[0052] The difference between this comparative example and Example 1 is that no inorganic flame retardant is added.

[0053] Add 0.5 g of sepiolite to 50 mL of deionized water, stir evenly, add 2 mL of 0.1 mol / L hydrochloric acid to adjust the pH to 4.6, stir at 12000 rpm for 30 min to obtain a suspension, add 3 g of polyvinyl alcohol to 30 mL of deionized water, stir at 90 ° C for 4 h, add to the suspension, stir for 2 h to obtain a mixture, spray the mixture evenly on glass wool, and solidify at 200 ° C for 15 min to obtain a glass wool felt loaded with sepiolite.

[0054] Example 2

[0055] The loaded modified glass wool felt aerogel is prepared by the following steps:

[0056] B1. Add 5g of tetraethyl orthosilicate to 25mL of ethanol and 75mL of deionized water, stir for 30min, add 3mL of 0.5mol / L hydrochloric acid, heat to 50°C, stir for 30min, let stand for 24h to fully hydrolyze tetraethyl orthosilicate, add 20mL of deionized water and 1mL of 60% ammonia water, stir for 30min, and obtain silica sol;

[0057] B2. Add 0.4g of modified glass wool felt to 15g of silica sol, and then add 15g of silica sol to just cover the glass wool felt, seal and age for 24h, add 20mL of deionized water and 80mL of ethanol for 12h, then add 2g of tetraethyl orthosilicate and 20mL of ethanol for secondary aging for 12h, add a mixed solution of isopropanol and n-hexane to replace the organic solvent, and then add a mixed solution of 2g of trimethylchlorosilane and 10mL of n-hexane for surface modification. When the gel becomes transparent, wash it 3 times with n-hexane and dry it in an oven at 60°C for 24h to obtain a loaded modified glass wool felt aerogel.

[0058] Comparative Example 3

[0059] The difference between this comparative example and Example 2 is that the modified glass wool felt is replaced by the material prepared in Comparative Example 1.

[0060] Comparative Example 4

[0061] The difference between this comparative example and Example 2 is that the modified glass wool felt is replaced by the material prepared in Comparative Example 2.

[0062] Comparative Example 5

[0063] The difference between this comparative example and Example 2 is that no silica sol is added.

[0064] Example 3

[0065] The modified polystyrene particles are prepared by the following steps:

[0066] Add 0.5g of zinc hydroxystannate to 40g of ethylene-vinyl acetate copolymer emulsion, stir evenly, place in a mixer, heat to 100°C, mix for 30min, cool to room temperature, take out, and obtain a composite material; add 3g of the composite material to 50mL of ethanol, stir until the composite material is completely dissolved, add 30mL of deionized water to dilute, add 1.8g of polystyrene particles, stir evenly, filter, and dry in an oven at 80°C for 10min to obtain modified polystyrene particles.

[0067] Comparative Example 6

[0068] The difference between this comparative example and Example 3 is that zinc hydroxystannate is not added.

[0069] 40 g of ethylene-vinyl acetate copolymer emulsion was mixed with 30 mL of deionized water to absorb moisture, 1.8 g of polystyrene particles were added, stirred evenly, filtered, and dried in an oven at 80° C. for 10 min to obtain modified polystyrene particles.

[0070] Example 4

[0071] A method for preparing an indoor thermal insulation board comprises the following steps:

[0072] 82.5g of modified polystyrene particles, 14g of loaded modified glass wool felt aerogel, 3g of polycaprolactone and 0.5g of calcium stearate are mixed, stirred evenly, and extruded in a twin-screw extruder. Under the conditions of zone 1 temperature of 230°C, zone 2 temperature of 235°C, zone 3 temperature of 237°C, zone 4 temperature of 240°C, zone 5 temperature of 245°C, and rotation speed of 500rpm, polystyrene board particles are obtained through drawing, cooling and pelletizing. The polystyrene board particles are mixed with 4g of butane, added to the extruder for extrusion molding, and obtained as thermal insulation board.

[0073] Example 5

[0074] A method for preparing an indoor thermal insulation board comprises the following steps:

[0075] 84.5g of modified polystyrene particles, 16g of loaded modified glass wool felt aerogel, 4g of polycaprolactone and 1g of calcium stearate are mixed, stirred evenly, and extruded in a twin-screw extruder. Under the conditions of 230°C in zone 1, 235°C in zone 2, 237°C in zone 3, 240°C in zone 4, and 245°C in zone 5, and a rotation speed of 500rpm, polystyrene board particles are obtained through drawing, cooling and pelletizing. The polystyrene board particles are mixed with 5g of butane, added to an extruder for extrusion molding, and obtained as a thermal insulation board.

[0076] Example 6

[0077] A method for preparing an indoor thermal insulation board comprises the following steps:

[0078] 86.5g of modified polystyrene particles, 18g of loaded modified glass wool felt aerogel, 5g of polycaprolactone and 1.5g of calcium stearate are mixed, stirred evenly, and extruded in a twin-screw extruder. Under the conditions of zone 1 temperature of 230°C, zone 2 temperature of 235°C, zone 3 temperature of 237°C, zone 4 temperature of 240°C, zone 5 temperature of 245°C, and rotation speed of 500rpm, polystyrene board particles are obtained through drawing, cooling and pelletizing. The polystyrene board particles are mixed with 6g of butane, added to the extruder for extrusion molding, and obtained as thermal insulation board.

[0079] Comparative Example 7

[0080] The difference between this comparative example and Example 4 is that the loaded modified glass wool felt aerogel is replaced by the material prepared in Comparative Example 3.

[0081] Comparative Example 8

[0082] The difference between this comparative example and Example 4 is that the loaded modified glass wool felt aerogel is replaced by the material prepared in Comparative Example 4.

[0083] Comparative Example 9

[0084] The difference between this comparative example and Example 4 is that the loaded modified glass wool felt aerogel is replaced by the material prepared in Comparative Example 5.

[0085] Comparative Example 10

[0086] The difference between this comparative example and Example 4 is that the modified polystyrene particles are replaced by the material prepared in Comparative Example 6.

[0087] The performance of the thermal insulation boards prepared in Examples 4-6 and Comparative Examples 7-10 is now tested;

[0088] The impact strength of the insulation board is tested according to GB / T1843-2008 "Impact Strength of Plastic Cantilever Beam"; the tensile strength of the insulation board is tested according to GB / T29906-2013 "Material for External Insulation System of Molded Polystyrene Board Thin Plastering Exterior Wall";

[0089] The thermal conductivity of the insulation board is tested according to GB / T10294-2008 "Determination of Steady-State Thermal Resistance and Related Properties of Insulating Materials - Guarded Hot Plate Method"; the thermal conductivity of the insulation board at 25°C;

[0090] According to GB / T2408-2008 "Determination of Combustion Performance of Plastics", the oxygen index of the insulation board is tested, and then the flame retardant performance of the insulation board is measured; according to GB / T1034-2008 "Determination of Water Absorption of Plastics", the volume water absorption rate of the insulation board is tested, and the test results are shown in Table 1 below:

[0091] Table 1

[0092]

[0093]

[0094] It can be seen from the data in Table 1 that in Comparative Example 7, the thermal insulation board prepared by adding aerogel prepared without adding sepiolite to polystyrene has reduced thermal insulation performance and mechanical properties. This may be because polyvinyl alcohol penetrates into the internal space channel of the sepiolite, preventing the organic binder component of the glass wool felt from being easily thermally decomposed at high temperature, resulting in reduced thermal insulation performance, and sepiolite has better mechanical properties; in Comparative Example 8, the thermal insulation board prepared by adding aerogel prepared without adding inorganic flame retardant to polystyrene has reduced thermal insulation performance and flame retardant properties. This may be because the flame retardant is deposited on the surface of the glass wool felt, avoiding contact between the glass wool felts, increasing the specific surface area of ​​the glass wool felt, and improving the thermal insulation performance. Performance, and has good flame retardant properties; in Comparative Example 9, the glass wool felt formed by not adding silica sol is directly added to the insulation board, and its thermal insulation and water resistance are reduced. This may be because the direct contact between the modified glass wool felts is reduced, the thermal conductivity is reduced, and the aerogel has a lower thermal conductivity and better thermal insulation performance; Comparative Example 10 does not add zinc hydroxystannate to prepare the insulation board, and its thermal stability and mechanical properties are reduced. This may be because the introduction of zinc hydroxystannate makes a three-dimensional network structure, improves the thermal stability of the copolymer, and greatly increases the viscosity of the copolymer, increasing the bonding force between the polystyrene particles and the inorganic material, thereby improving the toughness and impact resistance of the insulation board.

[0095] The data in Table 1 show that the thermal insulation board prepared in Examples 4-6 not only has good thermal insulation performance and flame retardant performance, but also the inorganic filler can be better combined with the organic thermal insulation board. An inorganic flame retardant is deposited on the surface of the loaded sepiolite glass wool felt, impregnated into the silica sol, and sealed and aged to obtain a loaded modified glass wool felt aerogel; zinc hydroxystannate is mixed with ethylene-vinyl acetate copolymer emulsion to obtain a composite material, polystyrene particles are modified using the composite material, mixed with the loaded modified glass wool felt aerogel and a compatibilizer, stirred evenly, placed in a twin-screw extruder for extrusion, stretched, cooled, pelletized, and then mixed with a foaming agent, added to an extruder for extrusion molding, and the prepared thermal insulation board meets the test performance requirements, while the thermal insulation board prepared in Comparative Examples 7-10 does not meet the performance requirements, indicating that the thermal insulation board prepared by the present invention not only has good thermal insulation performance and flame retardant performance, but also the inorganic filler can be better combined with the organic thermal insulation board.

[0096] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0097] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing an indoor thermal insulation board, characterized in that: The following steps are involved: S1. Using sepiolite to adsorb polyvinyl alcohol, coating it on the surface of glass wool, curing and molding to obtain a sepiolite-loaded glass wool felt, and depositing an inorganic flame retardant on the surface of the sepiolite-loaded glass wool felt to obtain a modified glass wool felt; S2. The modified glass wool felt is impregnated into the silica sol, and then sealed and aged to obtain a loaded modified glass wool felt aerogel; S3. The zinc hydroxystannate is mixed with an ethylene-vinyl acetate copolymer emulsion to obtain a composite material, and the composite material is used to modify polystyrene particles to obtain modified polystyrene particles; S4. The modified polystyrene particles, loaded modified glass wool felt aerogel and compatibilizer are mixed, stirred evenly, placed in a twin-screw extruder for extrusion, and subjected to drawing, cooling and pelletizing to obtain polystyrene board particles. The polystyrene board particles are mixed with a foaming agent, added to an extruder for extrusion molding to obtain a thermal insulation board.

2. The method for preparing an indoor thermal insulation board according to claim 1, characterized in that: The modified glass wool felt is prepared by the following steps: A1. Add sepiolite to deionized water, stir evenly, add 0.1 mol / L hydrochloric acid to adjust the pH to 4.6, stir at 12000 rpm for 30 min to obtain a suspension, add polyvinyl alcohol to deionized water, stir for 4 h, add to the suspension to obtain a mixture, spray the mixture evenly on glass wool, and cure at 200 ° C for 15 min to obtain a glass wool felt loaded with sepiolite; A2. Add the inorganic flame retardant to the ethanol solution and stir evenly to obtain a dispersion. Spray the dispersion on the surface of the loaded sepiolite glass wool felt and dry it in an oven at 80°C for 30 minutes to obtain a modified glass wool felt.

3. The method for preparing an indoor thermal insulation board according to claim 2, characterized in that: In the step A1, the ratio of sepiolite to hydrochloric acid is (0.3-0.7) g: (1-3) mL.

4. The method for preparing an indoor thermal insulation board according to claim 2, characterized in that: The inorganic flame retardant is one of aluminum hydroxide, magnesium hydroxide and red phosphorus, and has a particle size of 30-40 nm.

5. The method for preparing an indoor thermal insulation board according to claim 1, characterized in that: The loaded modified glass wool felt aerogel is prepared by the following steps: B1. Add ethyl orthosilicate to ethanol and deionized water, stir for 30 minutes, add 0.5 mol / L hydrochloric acid, heat to 50°C, stir for 30 minutes, let stand for 24 hours, add deionized water and 60% ammonia water, stir for 30 minutes, and obtain silica sol; B2. Add the modified glass wool felt to the silica sol, then add silica sol to cover the glass wool felt, seal and age for 24 hours, add deionized water and ethanol for 12 hours, then add tetraethyl orthosilicate and ethanol for secondary aging for 12 hours, add isopropanol and n-hexane to replace the solvent, stir, add trimethylchlorosilane and n-hexane when the gel becomes transparent, wash and dry to obtain the loaded modified glass wool felt aerogel.

6. The method for preparing an indoor thermal insulation board according to claim 5, characterized in that: In the step B2, the ratio of the modified glass wool felt to the silica sol is (0.2-0.6) g:(28-32) g.

7. The method for preparing an indoor thermal insulation board according to claim 1, characterized in that: The modified polystyrene particles are prepared by the following steps: The zinc hydroxystannate is added to the ethylene-vinyl acetate copolymer emulsion, stirred evenly, placed in a mixer, kneaded at 100° C. for 30 minutes, cooled, taken out, and a composite material is obtained; the composite material is added to ethanol, stirred, added with deionized water to dilute, and then polystyrene particles are added, stirred evenly, filtered, and dried to obtain modified polystyrene particles.

8. The method for preparing an indoor thermal insulation board according to claim 1, characterized in that: In the step S4, the compatibilizer is prepared by mixing polycaprolactone and calcium stearate in a mass ratio of (3-5) g:(0.5-1.5) g, and the foaming agent is butane.

9. The method for preparing an indoor thermal insulation board according to claim 1, characterized in that: In step S4, the temperature of the twin-screw extruder zone 1 is 230° C., the temperature of the zone 2 is 235° C., the temperature of the zone 3 is 237° C., the temperature of the zone 4 is 240° C., the temperature of the zone 5 is 245° C., and the main engine speed is 500 rpm.

10. The thermal insulation board obtained according to the preparation method according to any one of claims 1 to 9.