Environmentally friendly drag reducing agent for fracturing and preparation method thereof
By synthesizing nanoferrous tetraoxide, adsorbing cation exchange resin and grafting long-chain alkylamine monomer on the surface of molybdenum disulfide nanosheets, polymer drag reducing agents are solved in The antibacterial and dispersibility problems in high-temperature and water-based drag reducing agents have achieved efficient drag reduction effects and environmentally friendly characteristics.
Patent Information
- Application Number
- CN202411274945.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The antibacterial properties of polymer drag reducing agents are poor and are easily decomposed by bacterial microorganisms in the fracturing formation. In addition, polymers are used in high-temperature and high-mineralization reservoirs. The polymer molecular chain structure is thermally degraded, resulting in drag reduction. Performance declines; nanomaterials have poor dispersion in water-based drag reducing agents, which are prone to settlement and lead to a decline in drag reducing performance.
Synthesize nano iron tetroxide on the surface of molybdenum disulfide nanosheets to form a concave and convex structure to increase the heat transfer path and avoid high-temperature degradation; adsorb the cation exchange resin to the upper and lower surfaces of the modified molybdenum disulfide nanosheets to form a composite layered structure Fix metal ions to reduce binding to the drag reducing matrix; long-chain alkylamine monomers are grafted on the surface of layered nanomaterials to form a hydrophobic layer and improve dispersion; Caval structure using β-cyclodextrin is synergistic with amphiphilicity Drag reducer, reducing crude oil viscosity and shear stress.
It improves the temperature resistance, shear resistance and dispersion of the drag reducer, enhances the slip effect on the water flow, improves the recovery rate, and has good antibacterial activity and environmental protection characteristics.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of drag reducers for oil fields, in particular to an environmentally friendly drag reducer for fracturing and a preparation method thereof. Background Art
[0002] Low permeability reservoirs are rich in oil and gas reserves, and the formation pressure is high in the early stage of development. Usually, elastic exploitation is the main method. For general reservoirs, water injection development can achieve effective exploitation results. However, for water injection measures in low permeability reservoirs, the injection volume is low, the liquid production is low, and the recovery rate is low. It is easy to have high resistance and injection failure. If high-pressure water injection is forced, the ground equipment and downhole tools are easily damaged by high pressure, causing economic losses. Therefore, it is necessary to add an active agent to assist in reducing the injection pressure. Drag reducers are used to enhance water well injection. Active drag reduction and injection technology is one of the effective means to deal with the difficulties in water injection in low permeability reservoirs. The mechanism of action is to reduce the oil-water interface tension and boundary layer thickness, and improve the seepage capacity of the oil-water phase.
[0003] Polymer drag reducers have the characteristics of good drag reduction effect, small dosage and strong adaptability. They are widely used in slick water fracturing fluids. However, polymer drag reducers have poor antibacterial properties and are easily decomposed by bacterial microorganisms in fracturing formations. In addition, when polymers are used in high-temperature and high-mineralization oil reservoirs, the polymer molecular chain structure is destroyed by thermal degradation, resulting in a decrease in drag reduction performance. Nanomaterials are added to the drag reducer matrix, and small-sized, high-specific surface area nanoparticles can be efficiently adsorbed on the core surface to construct a hydrophobic and oleophobic surface structure, effectively improving the drag reduction effect. However, nanomaterials have poor dispersibility in water-based drag reducers and are prone to sedimentation, resulting in a decrease in drag reduction performance. Summary of the invention
[0004] The purpose of the present invention is to provide an environmentally friendly drag reducer for fracturing and a preparation method thereof: synthesizing nano-ferroferric oxide on the surface of molybdenum disulfide nanosheets, and then forming a concave-convex structure on the surface of the molybdenum disulfide nanosheets, increasing the heat transfer path, creating obstacles for heat transfer, and avoiding high-temperature degradation of the drag reducer matrix; cation exchange resin is adsorbed on the upper and lower surfaces of the modified molybdenum disulfide nanosheets, and graphene oxide acts on the surface of the modified molybdenum disulfide nanosheets to form a nano material with a composite layered structure, which has a higher capacity, and the cation exchange resin can react with K in the oil well. + , Ca 2+ , Fe 3+Cationic exchange occurs, fixing metal ions between layers of layered nanomaterials to avoid binding with the drag reducer matrix and reduce drag reduction performance; long-chain alkylamine monomers are grafted onto the surface of layered nanomaterials to form a hydrophobic layer on the surface of the reservoir rock wall, thereby producing a nano-slip effect on the water flow and achieving a drag reduction effect; the cavity structure contained in β-cyclodextrin has hydrophobic properties and can cooperate with the hydrophobic components of the amphiphilic drag reducer to adsorb on the hydrophobic chains of crude oil, weakening the π-π stacking force and van der Waals force between crude oil molecules, reducing crude oil viscosity and shear stress, and improving recovery.
[0005] The technical problems to be solved by the present invention are as follows: the antibacterial performance of polymer drag reducers is poor and they are easily decomposed by bacterial microorganisms in fracturing formations. Moreover, when polymers are used in high-temperature and high-mineralization oil reservoirs, the polymer molecular chain structure is destroyed by thermal degradation, resulting in a decrease in drag reduction performance. Nanomaterials are added to the drag reducer matrix, and small-sized, high-specific surface area nanoparticles can be efficiently adsorbed on the core surface to construct a hydrophobic and oleophobic surface structure, effectively improving the drag reduction effect. However, nanomaterials have poor dispersibility in water-based drag reducers and are prone to sedimentation, resulting in a decrease in drag reduction performance.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] An environmentally friendly drag reducer for fracturing comprises the following raw materials in parts by weight: 30-40 parts of acrylamide, 20-30 parts of acrylic acid, 5-10 parts of composite layered nano materials, 3-5 parts of antibacterial agents, 2-3 parts of surfactants, 0.1-0.3 parts of initiators and 50-60 parts of deionized water.
[0008] A method for preparing an environmentally friendly drag reducer for fracturing, comprising the following steps:
[0009] Acrylamide, acrylic acid, antibacterial agent and deionized water are mixed and stirred, and composite layered nanomaterials, surfactants and initiators are added. After heating and stirring for 10-20 minutes, after the reaction is completed, an environmentally friendly drag reducer for fracturing is obtained.
[0010] Furthermore, the surfactant is any one of sorbitan stearate, nonylphenol polyoxyethylene ether, and sorbitol polyoxyethylene ether.
[0011] Furthermore, the initiator is selected from any one of sodium hydroxide, azobiscyclohexylcarbonitrile and azobisisoheptanenitrile.
[0012] Furthermore, the stirring temperature is raised to 60-80°C.
[0013] Furthermore, the composite layered nanomaterial is prepared by modifying the surface of the layered nanomaterial with a long-chain alkylamine monomer.
[0014] Furthermore, the long-chain alkylamine is selected from any one of dodecylamine, tetradecylamine, hexadecylamine and octadecylamine.
[0015] Furthermore, the composite layered nanomaterial is specifically prepared by the following steps:
[0016] The layered nanomaterial is added to deionized water and stirred evenly to obtain a dispersion. The long-chain alkylamine is added to ethanol and stirred evenly. The dispersion is placed in the dispersion and stirred to react at 60°C for 12 hours. After the reaction is completed, it is filtered, washed with ethanol three times to remove unreacted long-chain alkylamine, washed with deionized water three times, and dried in an oven at 60°C for 10 minutes to obtain a composite layered nanomaterial.
[0017] Among them, the amine group of the long-chain alkylamine monomer can undergo an amidation reaction with the carboxyl group and epoxy group of graphene oxide in the layered nanomaterial, thereby grafting the long-chain alkylamine monomer on the surface of the layered nanomaterial, converting the hydrophilic layered nanomaterial into a hydrophobic one, and allowing the layered nanomaterial containing the remaining oxygen-containing functional groups and amide bonds to be chemically adsorbed onto the surface of the reservoir rock wall.
[0018] Furthermore, the amount ratio of the layered nanomaterial, deionized water, long-chain alkylamine, and ethanol is (1-2) g: (80-120) mL: (0.1-0.3) g: (45-55) mL.
[0019] Furthermore, the layered nanomaterial is prepared by modifying molybdenum disulfide nanosheets with catecholamines and then mixing them with cation exchange resin and graphene oxide.
[0020] Furthermore, the cation exchange resin is selected from D113 resin or 732 cation exchange resin.
[0021] Furthermore, the graphene oxide has a particle size of 0.5-1 μm and a thickness of 20-30 nm.
[0022] Further, the layered nanomaterial is specifically prepared by the following steps:
[0023] A1. Add modified molybdenum disulfide nanosheets into deionized water, disperse by ultrasound for 10 minutes, add Tris and 5% hydrochloric acid to adjust the pH to 8.5, stir, add 0.3 g of catecholamine, stir at room temperature for 24 hours, filter, wash with deionized water for 3 times, and dry in an oven at 60°C for 10 minutes to obtain solid particles.
[0024] Among them, catecholamines are used to modify the modified molybdenum disulfide nanosheets, so that the modified molybdenum disulfide nanosheets have excellent adhesion, and can adsorb cation exchange resins and graphene oxide to the surface of the modified molybdenum disulfide nanosheets, which is beneficial to the construction of layered composite materials.
[0025] Furthermore, the dosage ratio of modified molybdenum disulfide nanosheets, deionized water, Tris, hydrochloric acid, and catecholamines is (1.1-1.3) g: (45-55) mL: (0.04-0.08) g: (0.1-0.3) mL: (0.2-0.4) g.
[0026] A2. Add solid particles and cation exchange resin to ethanol, stir for 10 minutes, add graphene oxide, ultrasonically disperse for 30 minutes, stir at 85°C until the organic solvent evaporates, wash with deionized water three times, and dry in an oven at 60°C for 10 minutes to obtain a layered nanomaterial.
[0027] Among them, the modified molybdenum disulfide nanosheets grafted with catecholamines have good adhesion and can adsorb cation exchange resins to the upper and lower surfaces of the modified molybdenum disulfide nanosheets. The cationic groups carried by the cation exchange resins can be electrostatically bonded to the oxygen-containing functional groups on the surface of graphene oxide. Ultrasound helps graphene oxide to act on the surface of modified molybdenum disulfide nanosheets to form a nanomaterial with a composite layered structure.
[0028] Furthermore, the usage ratio of solid particles, cation exchange resin, ethanol and graphene oxide is (0.3-0.7) g:(2-3) g:(45-55) mL:(0.2-0.4) g.
[0029] Furthermore, the modified molybdenum disulfide nanosheets are prepared by mixing the molybdenum disulfide nanosheets with an iron source and subjecting the mixture to a hydrothermal treatment.
[0030] Furthermore, the particle size of the molybdenum disulfide nanosheets is 0.1-0.3 μm and the thickness is 10-20 nm.
[0031] Furthermore, the iron source is selected from any one of green vanadium, ferrous chloride and ferrous oxalate.
[0032] Furthermore, the hydrothermal treatment temperature is 160-180°C, and the hydrothermal treatment time is 10-12h.
[0033] Furthermore, the modified molybdenum disulfide nanosheets are specifically prepared by the following steps:
[0034] The iron source and molybdenum disulfide nanosheets were added to deionized water, stirred evenly, nitrogen was introduced, stirred at 60°C, hydrogen peroxide and a 2 mol / L sodium hydroxide aqueous solution were added to adjust the pH to 12, stirred for 15 minutes, placed in a reactor, and hydrothermally treated at 170°C for 12 hours. The mixture was cooled to room temperature, and the solid was collected by filtration. The solid was washed three times with deionized water and dried in an oven at 70°C for 15 minutes to obtain modified molybdenum disulfide nanosheets.
[0035] Among them, the oxygen-containing functional groups on the surface of molybdenum disulfide can combine with ferrous ions in the iron source, so that the ferrous ions are adsorbed to the surface of molybdenum disulfide nanosheets. After hydrothermal treatment, nano-ferroferric oxide can be synthesized on the surface of molybdenum disulfide nanosheets, and then a concave-convex structure is formed on the surface of molybdenum disulfide nanosheets, which increases the heat transfer path, creates obstacles for heat transfer, and avoids high-temperature degradation of the drag reducer matrix.
[0036] Furthermore, the dosage ratio of the iron source, molybdenum disulfide nanosheets, deionized water, hydrogen peroxide, and sodium hydroxide aqueous solution is (4-5) g: (0.3-0.7) g: (40-50) mL: (10-20) mL: (0.1-0.3) mL.
[0037] Furthermore, the antibacterial agent is prepared by reacting chitosan with hydroxypropyl-β-cyclodextrin, and then reacting with glycidyl trimethylammonium chloride and acrylic acid.
[0038] Furthermore, the average molecular weight of chitosan is 22.5-23.6 kDa, and the degree of deacetylation is 70.1-73.5%.
[0039] Furthermore, the antibacterial agent is specifically prepared by the following steps:
[0040] B1. Add chitosan to an aqueous solution of acetic acid with a mass fraction of 1%, stir evenly to obtain a mixed solution, mix hydroxypropyl-β-cyclodextrin with N,N-dimethylformamide, add the mixed solution, stir at 100°C for 24 hours, dialyze with a cellulose membrane with a molecular weight cutoff of 3500 kDa for 3 days, and freeze-dry at -20°C for 30 minutes to obtain modified hydroxypropyl-β-cyclodextrin.
[0041] Among them, the amino group of chitosan can react with the hydroxyl group of β-cyclodextrin, so that chitosan is grafted on β-cyclodextrin. Chitosan contains a large number of hydroxyl groups, which serve as reaction sites for quaternary ammonium salts, thereby realizing quaternized β-cyclodextrin with antibacterial activity.
[0042] Furthermore, the amount ratio of chitosan, acetic acid aqueous solution, hydroxypropyl-β-cyclodextrin, and N,N-dimethylformamide is (0.5-1.5) g: (70-90) mL: (2-4) g: (3-5) mL.
[0043] B2. Add modified hydroxypropyl-β-cyclodextrin to 1% acetic acid aqueous solution, stir evenly, add glycidyltrimethylammonium chloride, stir and react at 60°C for 2 hours, dialyze for 3 days, freeze-dry at -20°C for 30 minutes to obtain a solid, mix the solid with acrylic acid, add 36% hydrochloric acid, stir and react at 60°C for 10 minutes, filter, wash 3 times with deionized water, and dry in an oven at 60°C for 10 minutes to obtain an antibacterial agent.
[0044] Among them, the hydroxyl group of chitosan in the modified hydroxypropyl-β-cyclodextrin can undergo a ring-opening reaction with glycidyl trimethylammonium chloride to achieve quaternized β-cyclodextrin, which has antibacterial activity, kills bacteria during oil extraction, reduces pipeline corrosion, formation blockage, and drag reducer deterioration caused by bacteria; and the carboxyl group contained in acrylic acid can also undergo an esterification reaction with the hydroxyl group of modified hydroxypropyl-β-cyclodextrin, carries a reactive functional group, can copolymerize with the drag reducer matrix, and graft the modified antibacterial agent onto the polymer drag reducer molecular chain.
[0045] Furthermore, the usage ratio of modified hydroxypropyl-β-cyclodextrin, acetic acid aqueous solution, and glycidyltrimethylammonium chloride is (0.5-1.5) g: (70-90) mL: (5-7) mL.
[0046] Furthermore, the usage ratio of solid, acrylic acid and hydrochloric acid is (0.3-0.7) g:(8-12) mL:(0.1-0.2) mL.
[0047] Furthermore, compared with the prior art, the present invention has the following beneficial effects:
[0048] (1) In the technical solution of the present invention, molybdenum disulfide nanosheets are two-dimensional layered nanomaterials with weak van der Waals forces between layers, which can produce a rolling effect and have good lubricity. Nano-iron tetroxide is synthesized on the surface of the molybdenum disulfide nanosheets, and then a concave-convex structure is formed on the surface of the molybdenum disulfide nanosheets, which increases the heat transfer path, creates obstacles for heat transfer, and avoids high-temperature degradation of the drag reducer matrix.
[0049] (2) In the technical solution of the present invention, the cation exchange resin is adsorbed onto the upper and lower surfaces of the modified molybdenum disulfide nanosheets, and the cationic groups carried by the cation exchange resin can be electrostatically bonded with the oxygen-containing functional groups on the surface of graphene oxide, so that the graphene oxide acts on the surface of the modified molybdenum disulfide nanosheets to form a nanomaterial with a composite layered structure. On the one hand, the layered nanomaterial has a high capacity between the layers, and the cation exchange resin can bind to the K in the oil well. + , Ca 2+ , Fe 3+ Cationic exchange occurs, fixing the metal ions between the layers of the layered nanomaterials to avoid combining with the drag reducer matrix and reducing the drag reduction performance. On the other hand, the layered nanomaterials have a small size effect and can combine with the molecular chains of the drag reducer matrix to form a hybrid network structure, thereby improving the structural strength, temperature resistance and shear resistance of the drag reduction system.
[0050] (3) In the technical solution of the present invention, long-chain alkylamine monomers are grafted onto the surface of layered nanomaterials to convert the hydrophilic layered nanomaterials into hydrophobic ones. The layered nanomaterials containing the remaining oxygen-containing functional groups and amide bonds can be chemically adsorbed onto the surface of the reservoir rock wall to form a hydrophobic layer on the surface of the reservoir rock wall, thereby producing a nano-slip effect on the water flow, achieving a drag reduction effect, and improving the dispersibility of the layered nanomaterials to avoid agglomeration and performance degradation. In addition, it should be noted that the long-chain alkylamine monomers can be adsorbed onto the reservoir rock wall and the reservoir pore throat to form a hydrophobic layer, increase the entry of water flow, achieve water displacement of oil, and improve the recovery rate.
[0051] (4) In the technical scheme of the present invention, glycidyl trimethylammonium chloride is grafted onto hydroxypropyl-β-cyclodextrin through chitosan to achieve quaternized β-cyclodextrin, which has antibacterial activity and kills bacteria during oil production, thereby reducing pipeline corrosion, formation blockage, and drag reducer deterioration caused by bacteria; the antibacterial monomer reacts with acrylic acid, carries reactive functional groups, and can copolymerize with the drag reducer matrix, and the modified antibacterial agent is grafted onto the polymer drag reducer molecular chain to improve the antibacterial activity; the hydroxypropyl-β-cyclodextrin in the modified antibacterial monomer contains a cavity structure with hydrophobic properties, which can cooperate with the hydrophobic components of the amphiphilic drag reducer to be adsorbed on the hydrophobic chain of crude oil, weaken the π-π stacking force and van der Waals force between crude oil molecules, reduce crude oil viscosity and shear stress, and improve recovery rate.
[0052] (5) In the technical solution of the present invention, the drag reducing agent prepared by the present invention has good drag reducing performance, reduces energy consumption, is simple to prepare, has a short production cycle, meets environmental protection requirements, and has good antibacterial activity and heat stability. DETAILED DESCRIPTION
[0053] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0054] The raw materials used in the examples of the present invention are as follows: D113 resin (macroporous weakly acidic acrylic acid cation exchange resin, purchased from Yongzhou Water Treatment Technology Co., Ltd.); 732 cation exchange resin (crosslinking degree of 7%, molecular formula (C8H8) n, with -SO3H group on the benzene ring of the molecule, the resin is Na type during irradiation); green vanadium (99% content, Shandong Changyao New Materials Co., Ltd.); molybdenum disulfide nanosheets (Zhejiang Yamei Nanotechnology Co., Ltd., purity 99%); catecholamine (CAS: 59-92-7, Shanghai Jining Industrial Co., Ltd.); graphene oxide (Zhongke Leiming (Beijing) Technology Co., Ltd., content 99%); dodecylamine (content 99%, Tianjin Guangfu Fine Chemical Research Institute); chitosan (Beijing Jinming Biotechnology Co., Ltd.); hydroxypropyl-β-cyclodextrin (AR, Macklin's reagent); glycidyl trimethylammonium chloride (Guangzhou Weber Technology Co., Ltd.); N,N-dimethylformamide (Hubei Chengfeng Chemical Co., Ltd.); acrylic acid (M800E, Sinopec); hydrogen peroxide (Guangdong Xiaoda Chemical Co., Ltd.); Tris (a product of Shanghai Aladdin Reagent Company).
[0055] Example 1 The composite layered nanomaterial is prepared by the following steps:
[0056] A1. Add 4.36g of green vanadium and 0.5g of molybdenum disulfide nanosheets to 45mL of deionized water, stir evenly, introduce nitrogen, stir at 60°C, add 15mL of hydrogen peroxide and 0.2mL of 2mol / L sodium hydroxide aqueous solution to adjust the pH to 12, stir and react for 15min, place in a reactor, perform hydrothermal treatment at 170°C for 12h, cool to room temperature, filter and collect the solid, wash the solid three times with deionized water, and dry in an oven at 70°C for 15min to obtain modified molybdenum disulfide nanosheets.
[0057] A2. Add 1.2 g of modified molybdenum disulfide nanosheets to 50 mL of deionized water, disperse by ultrasonication for 10 min, add 0.06 g of Tris and 0.2 mL of 5% hydrochloric acid to adjust the pH to 8.5, stir, add 0.3 g of catecholamine, stir at room temperature for 24 h, filter, wash three times with deionized water, and dry in an oven at 60 ° C for 10 min to obtain solid particles.
[0058] A3. Add 0.5 g of solid particles and 2.6 g of D113 resin to 50 mL of ethanol, stir for 10 min, add 0.3 g of graphene oxide, ultrasonically disperse for 30 min, stir at 85 ° C until the organic solvent evaporates, wash three times with deionized water, and dry in an oven at 60 ° C for 10 min to obtain a layered nanomaterial.
[0059] A4.1.5g of layered nanomaterials were added to 100mL of deionized water and stirred to obtain a dispersion. 0.2g of dodecylamine was added to 50mL of ethanol and stirred to obtain a dispersion. The dispersion was placed in the dispersion and stirred to react at 60°C for 12h. After the reaction was completed, the mixture was filtered and washed with ethanol for 3 times to remove unreacted long-chain alkylamines. The mixture was washed with deionized water for 3 times and dried in an oven at 60°C for 10min to obtain a composite layered nanomaterial.
[0060] Comparative Example 1 The difference between this comparative example and Example 1 is that the modified molybdenum disulfide nanosheets are replaced by molybdenum disulfide nanosheets, and the remaining steps and raw materials are the same as Example 1.
[0061] A1. Add 1.2 g of molybdenum disulfide nanosheets to 50 mL of deionized water, ultrasonically disperse for 10 min, add 0.06 g of Tris and 0.2 mL of 5% hydrochloric acid to adjust the pH to 8.5, stir, add 0.3 g of catecholamine, stir at room temperature for 24 h, filter, wash three times with deionized water, and dry in an oven at 60 ° C for 10 min to obtain solid particles.
[0062] A2. Add 0.5 g of solid particles and 2.6 g of D113 resin to 50 mL of ethanol, stir for 10 min, add 0.3 g of graphene oxide, ultrasonically disperse for 30 min, stir at 85 ° C until the organic solvent evaporates, wash with deionized water three times, and dry in an oven at 60 ° C for 10 min to obtain a layered nanomaterial.
[0063] A3.1.5g of layered nanomaterials were added to 100mL of deionized water and stirred to obtain a dispersion. 0.2g of dodecylamine was added to 50mL of ethanol and stirred to obtain a dispersion. The dispersion was placed in the dispersion and stirred to react at 60°C for 12h. After the reaction was completed, the mixture was filtered and washed with ethanol for 3 times to remove unreacted long-chain alkylamines. The mixture was washed with deionized water for 3 times and dried in an oven at 60°C for 10min to obtain a composite layered nanomaterial.
[0064] Comparative Example 2 The difference between this comparative example and Example 1 is that D113 resin and graphene oxide are not added, and the remaining steps and raw materials are the same as Example 1.
[0065] A1. Add 4.36g of green vanadium and 0.5g of molybdenum disulfide nanosheets to 45mL of deionized water, stir evenly, introduce nitrogen, stir at 60°C, add 15mL of hydrogen peroxide and 0.2mL of 2mol / L sodium hydroxide aqueous solution to adjust the pH to 12, stir and react for 15min, place in a reactor, perform hydrothermal treatment at 170°C for 12h, cool to room temperature, filter and collect the solid, wash the solid three times with deionized water, and dry in an oven at 70°C for 15min to obtain modified molybdenum disulfide nanosheets.
[0066] A2.1.5g of modified molybdenum disulfide nanosheets were added to 100mL of deionized water and stirred to obtain a dispersion. 0.2g of dodecylamine was added to 50mL of ethanol and stirred to obtain a dispersion. The dispersion was placed in the dispersion and stirred to react at 60°C for 12h. After the reaction was completed, the nanosheets were filtered, washed with ethanol three times to remove unreacted long-chain alkylamine, washed with deionized water three times, and dried in an oven at 60°C for 10min to obtain nanomaterials.
[0067] Comparative Example 3 The difference between this comparative example and Example 1 is that no long-chain alkylamine monomer is added, and the remaining steps and raw materials are the same as those in Example 1.
[0068] A1. Add 4.36g of green vanadium and 0.5g of molybdenum disulfide nanosheets to 45mL of deionized water, stir evenly, introduce nitrogen, stir at 60°C, add 15mL of hydrogen peroxide and 0.2mL of 2mol / L sodium hydroxide aqueous solution to adjust the pH to 12, stir and react for 15min, place in a reactor, perform hydrothermal treatment at 170°C for 12h, cool to room temperature, filter and collect the solid, wash the solid three times with deionized water, and dry in an oven at 70°C for 15min to obtain modified molybdenum disulfide nanosheets.
[0069] A2. Add 1.2 g of modified molybdenum disulfide nanosheets to 50 mL of deionized water, disperse by ultrasonication for 10 min, add 0.06 g of Tris and 0.2 mL of 5% hydrochloric acid to adjust the pH to 8.5, stir, add 0.3 g of catecholamine, stir at room temperature for 24 h, filter, wash three times with deionized water, and dry in an oven at 60 ° C for 10 min to obtain solid particles.
[0070] A3. Add 0.5 g of solid particles and 2.6 g of D113 resin to 50 mL of ethanol, stir for 10 min, add 0.3 g of graphene oxide, ultrasonically disperse for 30 min, stir at 85 ° C until the organic solvent evaporates, wash three times with deionized water, and dry in an oven at 60 ° C for 10 min to obtain a composite layered nanomaterial.
[0071] Example 2 The antibacterial agent is prepared by the following steps:
[0072] B1. Add 1 g of chitosan to 80 mL of 1% acetic acid aqueous solution and stir evenly to obtain a mixed solution. Mix 3 g of hydroxypropyl-β-cyclodextrin with 4 mL of N,N-dimethylformamide, add the mixed solution, stir at 100°C for 24 h, dialyze with a cellulose membrane with a molecular weight cutoff of 3500 kDa for 3 days, and freeze-dry at -20°C for 30 min to obtain modified hydroxypropyl-β-cyclodextrin.
[0073] B2. Add 1g of modified hydroxypropyl-β-cyclodextrin to 80mL of 1% acetic acid aqueous solution, stir evenly, add 6mL of glycidyltrimethylammonium chloride, stir and react at 60℃ for 2h, dialyze for 3 days, freeze-dry at -20℃ for 30min to obtain a solid, mix 0.5g of the solid with 10mL of acrylic acid, add 0.15mL of 36% hydrochloric acid, stir and react at 60℃ for 10min, filter, wash with deionized water 3 times, and dry in an oven at 60℃ for 10min to obtain an antibacterial agent.
[0074] Comparative Example 4 The difference between this comparative example and Example 2 is that glycidyl trimethylammonium chloride and acrylic acid are not added, and the remaining steps and raw materials are the same as those in Example 2.
[0075] Add 1 g of chitosan to 80 mL of 1% acetic acid aqueous solution and stir evenly to obtain a mixed solution. Mix 3 g of hydroxypropyl-β-cyclodextrin with 4 mL of N,N-dimethylformamide and add the mixed solution. Stir at 100 °C for 24 h, dialyze with a cellulose membrane with a molecular weight cutoff of 3500 kDa for 3 days, and freeze-dry at -20 °C for 30 min to obtain modified hydroxypropyl-β-cyclodextrin.
[0076] Example 3 An environmentally friendly drag reducer for fracturing includes the following raw materials in parts by weight: 30 parts of acrylamide, 20 parts of acrylic acid, 5 parts of composite layered nanomaterials, 3 parts of antibacterial agent, 2 parts of nonylphenol polyoxyethylene ether, 0.1 parts of azobiscyclohexylcarbonitrile, and 50 parts of deionized water.
[0077] A method for preparing an environmentally friendly drag reducer for fracturing, comprising the following steps:
[0078] Acrylamide, acrylic acid, antibacterial agent and deionized water are mixed and stirred, and composite layered nanomaterials, nonylphenol polyoxyethylene ether and azobiscyclohexylcarbonitrile are added. The temperature is raised to 70° C. and stirred for 15 minutes. After the reaction is completed, an environmentally friendly drag reducer for fracturing is obtained.
[0079] Example 4 An environmentally friendly drag reducer for fracturing includes the following raw materials in parts by weight: 35 parts of acrylamide, 25 parts of acrylic acid, 8 parts of composite layered nanomaterials, 4 parts of antibacterial agent, 2.5 parts of sorbitan stearate, 0.2 parts of sodium hydroxide, and 55 parts of deionized water.
[0080] A method for preparing an environmentally friendly drag reducer for fracturing, comprising the following steps:
[0081] Acrylamide, acrylic acid, antibacterial agent and deionized water are mixed and stirred, and composite layered nanomaterials, sorbitan stearate and sodium hydroxide are added. The temperature is raised to 70° C. and stirred for 15 minutes. After the reaction is completed, an environmentally friendly drag reducer for fracturing is obtained.
[0082] Example 5 An environmentally friendly drag reducer for fracturing includes the following raw materials in parts by weight: 40 parts of acrylamide, 30 parts of acrylic acid, 10 parts of composite layered nanomaterials, 5 parts of antibacterial agent, 3 parts of sorbitol polyoxyethylene ether, 0.3 parts of azobisisoheptonitrile, and 60 parts of deionized water.
[0083] A method for preparing an environmentally friendly drag reducer for fracturing, comprising the following steps:
[0084] Acrylamide, acrylic acid, antibacterial agent and deionized water are mixed and stirred, and composite layered nanomaterials, sorbitol polyoxyethylene ether and azobisisoheptanenitrile are added. The temperature is raised to 70° C. and stirred for 15 minutes. After the reaction is completed, an environmentally friendly drag reducer for fracturing is obtained.
[0085] Comparative Example 5 The difference between this comparative example and Example 4 is that the composite layered nanomaterial is replaced by the material prepared in Comparative Example 1, and the remaining steps and raw materials are the same as those in Example 4.
[0086] Comparative Example 6 The difference between this comparative example and Example 4 is that the composite layered nanomaterial is replaced by the nanomaterial prepared in Comparative Example 2, and the remaining steps and raw materials are the same as those in Example 4.
[0087] Comparative Example 7 The difference between this comparative example and Example 4 is that the composite layered nanomaterial is replaced by the material prepared in Comparative Example 3, and the remaining steps and raw materials are the same as those in Example 4.
[0088] Comparative Example 8 The difference between this comparative example and Example 4 is that the antibacterial agent is replaced by the modified hydroxypropyl-β-cyclodextrin prepared in Comparative Example 4, and the remaining steps and raw materials are the same as those in Example 4.
[0089] The environmentally friendly drag reducers for fracturing prepared in Examples 3-5 and Comparative Examples 5-8 are now tested for their performance;
[0090] Mix 10 g of the environmentally friendly drag reducer for fracturing prepared above with 1000 g of water to obtain a drag reducer solution;
[0091] Drag reduction performance measurement: The drag reduction performance of the drag reducer solution was measured using an SLSY pipeline friction tester. The pipeline diameter was 8 mm, the test flow rate was 2 L / s, and the test temperature was 30 °C.
[0092] Shear resistance test: The drag reducer solution was tested for changes in apparent viscosity at different shear times using a DSR-1 dynamic shear rheometer at room temperature. The shear rate was 170 s / min and the shear time was 60 min.
[0093] Temperature resistance performance measurement: The thermal stability of the environmentally friendly drag reducer sample prepared above was analyzed using a thermogravimetric analyzer. 10g of the environmentally friendly drag reducer was taken, and the measurement temperature range was 0-800°C. N2 was used as an inert atmosphere. The weight loss of the sample was measured at a heating rate of 20°C / min, and the thermal weight loss data was recorded to determine the temperature resistance performance.
[0094] According to the Chinese petroleum and natural gas industry standard SY / T0532-1993 "Oilfield injection water bacteria analysis method - extinction dilution method", the antibacterial rate of environmentally friendly drag reducer used for fracturing was determined; the results are shown in Table 1 below:
[0095]
[0096] It can be seen from the data in Table 1 that in Comparative Example 5, the composite layered nanomaterial prepared by replacing the modified molybdenum disulfide nanosheets with molybdenum disulfide nanosheets is added to the drag reducer, and its drag reduction performance and temperature resistance are reduced. This may be because nano-iron tetroxide is synthesized on the surface of the molybdenum disulfide nanosheets, and then a concave-convex structure is formed on the surface of the molybdenum disulfide nanosheets, which increases the heat transfer path, creates obstacles for heat transfer, avoids high-temperature degradation of the drag reducer matrix, and improves the drag reduction performance; in Comparative Example 6, the nanomaterial prepared without adding D113 resin and graphene oxide is added to the drag reducer, and its drag reduction performance and shear resistance are reduced. This may be because the cation exchange resin can react with K in the oil well. + , Ca 2+ , Fe 3+ Cationic exchange occurs, and the metal ions are fixed between the layers of the layered nanomaterials to avoid combining with the drag reducer matrix, thereby reducing the drag reduction performance, and the layered nanomaterials can improve the shear resistance of the drag reduction system; in Example 7, the nanomaterial prepared without adding long-chain alkylamine monomers is added to the drag reducer, and its drag reduction performance and shear resistance are reduced. This may be because the long-chain alkylamine monomers are grafted on the surface of the layered nanomaterials and can be chemically adsorbed to the surface of the reservoir rock wall to form a hydrophobic layer on the surface of the reservoir rock wall, thereby producing a nano-slip effect on the water flow, achieving a drag reduction effect, and improving the dispersibility of the layered nanomaterials to avoid agglomeration and performance degradation; in Example 8, the antibacterial agent prepared without adding glycidyl trimethylammonium chloride and acrylic acid is added to the drag reducer, and its antibacterial performance is reduced. This may be because the quaternized β-cyclodextrin has antibacterial activity, the antibacterial monomer reacts with acrylic acid, carries reactive functional groups, can copolymerize with the drag reducer matrix, and the modified antibacterial agent is grafted on the molecular chain of the polymer drag reducer to improve the antibacterial activity.
[0097] The data in Table 1 show that the environmentally friendly drag reducers for fracturing prepared in Examples 3-5 meet the test performance requirements, while the environmentally friendly drag reducers for fracturing prepared in Comparative Examples 5-8 do not meet the performance requirements, indicating that the environmentally friendly drag reducers for fracturing prepared in the present invention have good temperature resistance, antibacterial activity and drag reduction performance.
[0098] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0099] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. An environmentally friendly drag reducer for fracturing, characterized in that: The raw materials include the following parts by weight: 30-40 parts of acrylamide, 20-30 parts of acrylic acid, 5-10 parts of composite layered nanomaterials, 3-5 parts of antibacterial agents, 2-3 parts of surfactants, 0.1-0.3 parts of initiators, and 50-60 parts of deionized water; The composite layered nanomaterial is prepared by surface-modifying a layered nanomaterial with a long-chain alkylamine monomer; The composite layered nanomaterial is specifically prepared by the following steps: The layered nanomaterial is added to deionized water and stirred evenly to obtain a dispersion, and a long-chain alkylamine is added to ethanol and stirred evenly, placed in the dispersion, and stirred for reaction at 60°C for 12 hours. After the reaction is completed, it is filtered, washed with ethanol three times to remove unreacted long-chain alkylamine, washed with deionized water three times, and dried in an oven at 60°C for 10 minutes to obtain a composite layered nanomaterial; The layered nanomaterial is prepared by modifying molybdenum disulfide nanosheets with catecholamines and then mixing them with cation exchange resin and graphene oxide; The layered nanomaterial is specifically prepared by the following steps: A1. Add the modified molybdenum disulfide nanosheets to deionized water, ultrasonically disperse for 10 minutes, add Tris and 5% hydrochloric acid to adjust the pH to 8.5, stir, add 0.3 g of catecholamine, stir at room temperature for 24 hours, filter, wash with deionized water three times, and dry in an oven at 60°C for 10 minutes to obtain solid particles; A2. The solid particles and cation exchange resin were added to ethanol, stirred for 10 minutes, and then graphene oxide was added. The mixture was ultrasonically dispersed for 30 minutes, stirred at 85°C until the organic solvent evaporated, washed with deionized water for 3 times, and dried in an oven at 60°C for 10 minutes to obtain a layered nanomaterial. The modified molybdenum disulfide nanosheets are prepared by mixing molybdenum disulfide nanosheets with an iron source and subjecting the mixture to a hydrothermal treatment; The antibacterial agent is prepared by reacting chitosan with hydroxypropyl-β-cyclodextrin, and then reacting with glycidyl trimethylammonium chloride and acrylic acid.
2. The environmentally friendly drag reducer for fracturing according to claim 1, characterized in that: The long-chain alkylamine is selected from any one of dodecylamine, tetradecylamine, hexadecylamine and octadecylamine.
3. The environmentally friendly drag reducer for fracturing according to claim 1, characterized in that: The cation exchange resin is selected from D113 resin or 732 cation exchange resin.
4. The environmentally friendly drag reducer for fracturing according to claim 1, characterized in that: The hydrothermal treatment temperature is 160-180° C., and the hydrothermal treatment time is 10-12 hours.
5. The environmentally friendly drag reducer for fracturing according to claim 1, characterized in that: The iron source is selected from any one of green vanadium, ferrous chloride and ferrous oxalate.
6. The environmentally friendly drag reducer for fracturing according to claim 5, characterized in that: The chitosan has an average molecular weight of 22.5-23.6 kDa and a deacetylation degree of 70.1-73.5%.
7. The environmentally friendly drag reducer for fracturing according to claim 1, characterized in that: The surfactant is any one of sorbitan stearate, nonylphenol polyoxyethylene ether and sorbitol polyoxyethylene ether.
8. The environmentally friendly drag reducer for fracturing according to claim 1, characterized in that: The initiator is selected from any one of sodium hydroxide, azobiscyclohexylcarbonitrile and azobisisoheptanenitrile.
9. The environmentally friendly drag reducer for fracturing according to claim 1, characterized in that: The graphene oxide has a particle size of 0.5-1 μm and a thickness of 20-30 nm; the molybdenum disulfide nanosheet has a particle size of 0.1-0.3 μm and a thickness of 10-20 nm.
10. The method for preparing an environmentally friendly drag reducer for fracturing according to any one of claims 1 to 9, characterized in that: The specific steps include: Acrylamide, acrylic acid, antibacterial agent and deionized water are mixed and stirred, and composite layered nanomaterials, surfactants and initiators are added. After heating and stirring for 10-20 minutes, after the reaction is completed, an environmentally friendly drag reducer for fracturing is obtained.