Chitosan-based antibacterial hemostatic material as well as preparation method and application thereof
By combining chitosan with attapulgite to form an A/LQC/CS sponge with porous structure and antibacterial activity, it solves the shortcomings of existing hemostatic materials in non-compressive penetrating injury bleeding and antibacterial, and achieves efficient hemostasis and Promote wound healing.
Patent Information
- Application Number
- CN202411312573.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hemostatic materials have limited hemostatic and antibacterial effects, and are particularly difficult to effectively treat non-compressive penetrating wounds with severe bleeding and bacterial infection.
An antibacterial hemostatic material based on chitosan is used. Chitosan is modified through quaternization and lauric acid, and combined with attapulgite to form an A/LQC/CS sponge with porous structure, high mechanical strength and antibacterial activity.
The material shows excellent results in non-compressive penetrating wound bleeding, has significant antibacterial activity, promotes wound healing, reduces inflammation, and significantly improves hemostasis and wound healing efficiency.
Smart Images

Figure CN118806971A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to medical material technology, and in particular to an antibacterial hemostatic material based on chitosan, and a preparation method and application thereof. Background Art
[0002] Wound healing includes four different sequential stages: hemostasis, inflammation, proliferation, and remodeling. An ideal hemostatic material should have strong hemostatic, antibacterial, and wound healing properties. Currently, most commercial hemostatic agents (such as gauze, fibrin-based bandages, QuickClot, and hemostatic particles) have limited hemostatic and antibacterial effects and are not suitable for hemostasis of non-compressive penetrating injuries. Therefore, it is urgent to develop a new hemostatic material with procoagulant and antibacterial activity that can be used for hemostasis of non-compressive penetrating injuries.
[0003] Chitosan is a cationic polysaccharide formed by deacetylation of chitin. It is well-known for its inherent procoagulant, antibacterial and wound healing properties and is an ideal matrix material for preparing hemostatic materials. Chitosan can be prepared into a porous sponge to concentrate blood, absorb excess wound exudate, transport nutrients and promote cell migration, etc. It has obvious advantages in wound repair. However, the procoagulant and antibacterial effects of pure chitosan sponge are limited, making it difficult to effectively treat wounds with severe bleeding and bacterial infection. Summary of the invention
[0004] The purpose of the present invention is to provide an antibacterial hemostatic material based on chitosan and a preparation method and application thereof, so as to solve the above-mentioned deficiencies in the prior art.
[0005] In order to achieve the above-mentioned purpose, the present invention provides the following technical scheme: an antibacterial hemostatic material based on chitosan, comprising the antibacterial hemostatic material being an A / LQC / CS sponge, the A / LQC / CS sponge comprising three components: chitosan, lauric acid-modified quaternary ammonium chitosan and attapulgite, and the mass ratio of the chitosan to the lauric acid-modified quaternary ammonium chitosan is 4:1.
[0006] A method for preparing an antibacterial hemostatic material based on chitosan, which is applicable to an antibacterial hemostatic material based on chitosan, comprises the following steps: S1, firstly preparing quaternized chitosan; S2, then preparing lauric acid modified quaternary ammonium chitosan; S3. Finally, prepare A / LQC / CS sponge.
[0007] Furthermore, the preparation of the quaternized chitosan described in S1 comprises the following steps: S11, dispersing chitosan in deionized water, adding glacial acetic acid and stirring to obtain a chitosan solution; S12, dissolving 2,3-epoxypropyltrimethylammonium chloride in deionized water, adding the 2,3-epoxypropyltrimethylammonium chloride solution dropwise into the chitosan solution for reaction, placing the reaction solution into a dialysis bag, dialyzing it in deionized water, and freeze-drying it to obtain quaternized chitosan.
[0008] Furthermore, the preparation of the lauric acid modified quaternary ammonium chitosan described in S2 comprises the following steps: S21, dissolving QCS in deionized water, dissolving carbodiimide hydrochloride, N-hydroxysuccinimide and lauric acid in methanol for activation, dropping the QCS solution into the activation solution, and reacting at room temperature; S22, putting the reaction solution into a dialysis bag, dialyzing it in deionized water, and freeze-drying it to obtain lauric acid-modified quaternary ammonium chitosan.
[0009] Further, the preparation of the A / LQC / CS sponge described in S3 comprises the following steps: S31, firstly preparing LQC / CS sponge; S32. Finally, prepare A / LQC / CS sponge.
[0010] Further, the preparation of LQC / CS sponge in S31 comprises the following steps: Chitosan and lauric acid-modified quaternized chitosan were dissolved in an acetic acid aqueous solution to obtain a composite solution, which was then centrifuged and poured into a mold, and finally freeze-dried to prepare an LQC / CS sponge.
[0011] Further, the preparation of the A / LQC / CS sponge described in S32 comprises the following steps: The LQC / CS sponge was soaked in an ethanol / sodium hydroxide solution and then washed with water. After washing, the LQC / CS sponge was compressed and placed in a attapulgite suspension to obtain an LQC / CS sponge loaded with attapulgite, namely, A / LQC / CS sponge.
[0012] Furthermore, the mass volume percentage of attapulgite in the attapulgite suspension is 3%.
[0013] The invention discloses an application of an antibacterial hemostatic material based on chitosan in the preparation of a medical hemostatic sponge.
[0014] Application of the chitosan-based antibacterial hemostatic material prepared by the preparation method in the preparation of medical hemostatic sponge.
[0015] Compared with the prior art, the present invention provides an antibacterial hemostatic material based on chitosan, a preparation method thereof and an application thereof. The sponge has an interconnected porous structure, high self-elasticity, high mechanical strength, rapid shape recovery ability and strong ability to promote blood cell adhesion, aggregation and activation, and activate endogenous / exogenous coagulation cascade reactions. In addition, the sponge shows excellent effects in treating non-compressive liver penetrating wound bleeding, and shows significant antibacterial activity against Staphylococcus aureus, Escherichia coli and methicillin-resistant Staphylococcus aureus. The sponge has good biocompatibility and biosafety. The sponge can promote wound healing by accelerating re-epithelialization and collagen deposition, reducing inflammation and promoting angiogenesis, showing a wound healing effect superior to commercial dressings, and can be used in the preparation of medical hemostatic sponges. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.
[0017] Figure 1 A schematic diagram of the preparation process of A / LQC / CS sponge provided in an embodiment of the present invention; Figure 2 The preparation process and related spectral characterization diagram of lauric acid modified quaternary ammonium chitosan provided in the embodiment of the present invention; Figure 3 Characterization diagram of A / LQC / CS sponge provided in an embodiment of the present invention; Figure 4 A schematic diagram of the elasticity and shape recovery performance of the A / LQC / CS sponge provided in an embodiment of the present invention; Figure 5 A schematic diagram of the procoagulant performance of the A / LQC / CS sponge provided in an embodiment of the present invention; Figure 6 A schematic diagram of the hemostatic performance of the A / LQC / CS sponge provided in an embodiment of the present invention; Figure 7 Schematic diagram of the antibacterial performance of the A / LQC / CS sponge provided in an embodiment of the present invention; Figure 8 A schematic diagram of the biocompatibility and biosafety of the A / LQC / CS sponge provided in an embodiment of the present invention; Fig. 9 Schematic diagram of the wound healing promoting ability of the A / LQC / CS sponge provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0018] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.
[0019] Embodiment 1:
[0020] See also Figure 1-Figure 9 , an antibacterial hemostatic material based on chitosan, the antibacterial hemostatic material is A / LQC / CS sponge, A / LQC / CS sponge includes three components: chitosan, lauric acid modified quaternary ammonium chitosan and attapulgite, and the mass ratio of chitosan and lauric acid modified quaternary ammonium chitosan is 4:1.
[0021] The specific implementation method is that chitosan (CS) is a natural polysaccharide with good biocompatibility and degradability. It can be degraded by lysozyme in the body into glucosamine and N-acetylglucosamine required by the body, and will not cause adverse reactions to the human body; chitosan can promote the growth of normal fibroblasts and epithelial cells, accelerate wound healing, and activate related cells in wound healing, such as macrophages, white blood cells, etc., to promote wound healing in a timely manner. These cells play a key role in the wound healing process, and can remove necrotic tissue and promote the formation of new tissue.
[0022] Attapulgite (A) has a large specific surface area and micro-mesoporous structure, which enables it to effectively adsorb and concentrate coagulation factors in the blood, such as platelets, red blood cells, etc. This adsorption ability helps to quickly form blood clots at the wound, thereby achieving the effect of hemostasis. Attapulgite not only has physical adsorption ability, but also may interact with coagulation factors in the blood through chemical groups on its surface to activate endogenous coagulation. Attapulgite can induce platelet contact activation and promote platelet aggregation and coagulation, which is a crucial step in the hemostasis process. In addition, attapulgite containing negatively charged silanol groups can interact with positively charged polymers to enhance the mechanical strength of the material.
[0023] Quaternized and alkylated polymers have been shown to have strong procoagulant ability and broad-spectrum antibacterial activity, which is attributed to the electrostatic and hydrophobic interactions between the positively charged quaternary ammonium groups and hydrophobic alkyl chains and the blood cell / bacterial membrane, promoting the adhesion, aggregation and activation of blood cells, destroying the integrity of the biofilm, and leading to bacterial death.
[0024] Embodiment 2:
[0025] See also Figure 1-Figure 2 This embodiment provides a technical solution based on the first embodiment: a method for preparing an antibacterial hemostatic material based on chitosan, which is applicable to an antibacterial hemostatic material based on chitosan, comprising the following steps: S1, firstly preparing quaternized chitosan; Disperse 4 g of chitosan in 144 mL of deionized water, add 720 μL of glacial acetic acid, and stir at room temperature for 8 h to obtain a chitosan solution; Dissolve 6.4 g of 2,3-epoxypropyltrimethylammonium chloride in 40 mL of deionized water to obtain a 2,3-epoxypropyltrimethylammonium chloride solution; Then, 2,3-epoxypropyltrimethylammonium chloride solution was added dropwise to the chitosan solution, reacted at 55°C for 24 hours, the reaction solution was put into a dialysis bag (molecular weight cutoff of 8-14 kDa), dialyzed in deionized water for 3 days, and freeze-dried after the dialysis was completed to obtain quaternary ammonium chitosan (QCS).
[0026] S2, then preparing lauric acid modified quaternary ammonium chitosan; 0.5 g of QCS was dissolved in 50 mL of deionized water, and carbodiimide hydrochloride (EDC·HCl), N-hydroxysuccinimide (NHS), and lauric acid were dissolved in methanol and activated for 1 h; The QCS solution was added dropwise to the activation solution, and after reacting at room temperature for 48 hours, the reaction solution was placed in a dialysis bag (molecular weight cutoff of 8-14 kDa), dialyzed in deionized water for 3 days, and freeze-dried to obtain lauric acid-modified quaternary ammonium chitosan (LQC).
[0027] Fourier transform infrared spectrometer (ATR-FTIR) and hydrogen nuclear magnetic resonance (H-NMR) 1 H NMR) to characterize the chemical structure of the product.
[0028] S3, finally preparing A / LQC / CS sponge; 4 g CS and 1 g LQC were dissolved in 100 mL acetic acid aqueous solution (2%, v / v) to prepare a composite solution. After centrifugation at 8000 rpm for 3 min, the composite solution was poured into a mold, cooled to -20°C at a rate of 1°C / min, and then freeze-dried to prepare an LQC / CS sponge. The LQC / CS sponge was soaked in ethanol / sodium hydroxide solution to neutralize the excess acetic acid. After neutralization, it was rinsed with water. Then, the LQC / CS sponge was compressed and placed in a 3% (w / v) attapulgite suspension for 4 h to prepare the A / LQC / CS sponge.
[0029] Embodiment three:
[0030] See also Figure 2-Figure 3 This embodiment provides a technical solution based on the second embodiment: using ATR-FTIR and 1 The chemical structures of QCS and LQC were characterized by H NMR. The microstructure and chemical composition of the sponges were analyzed by scanning electron microscopy and energy dispersive spectroscopy.
[0031] See also Figure 2 , QCS was synthesized by the ring-opening reaction between the amino group of CS and the epoxy group of GTMAC. In the ATR-FTIR spectrum of QCS, 1642, 1555, and 1260 cm -1 The characteristic peaks at 1476 cm-1 are attributed to amide I, amide II, and amide III in CS. −1 The characteristic peak at is attributed to the trimethylammonium group in GTMAC. 1 In the H NMR spectrum, the characteristic peaks at 4.56 and 3.28 ppm were attributed to the methylene hydrogen protons in CS and the methyl hydrogen protons in GTMAC, respectively. The above results proved the successful synthesis of QCS. The substitution degree of QCS was about 34.4%. Secondly, LQC was synthesized by the amidation reaction between the amino group of LQC and the carboxyl group of lauric acid. 1 In the H NMR spectrum, the characteristic peaks at 4.54 and 3.26 ppm were attributed to the methine hydrogen protons in CS and the methyl hydrogen protons in GTMAC, respectively, and the characteristic peak at 0.87 ppm was attributed to the methyl hydrogen protons in lauric acid, which proved the successful synthesis of LQC. The degree of substitution of LQC was about 7.0%.
[0032] See also Figure 3 , LQC / CS sponge was prepared by freeze-drying the cooled LQC / CS solution, and then attapulgite was adsorbed into the LQC / CS sponge to prepare A / LQC / CS sponge. In the ATR-FTIR spectrum of LQC / CS sponge, the -1 The characteristic peaks attributed to the quaternary ammonium (trimethylammonium) group in LQC were observed at , proving the successful composite of LQC and CS. Compared with CS and LQC / CS sponges, the color of A / LQC / CS sponge is gray-brown, and its pore walls are relatively rough (loaded attapulgite), proving the successful loading of attapulgite. Attapulgite, also known as attapulgite or rod crystal, is a natural hydrated magnesium aluminum silicate mineral with a special structure. In the energy dispersive spectrum of A / LQC / CS sponge, carbon (C), oxygen (O), aluminum (Al) and silicon (Si) elements are evenly distributed on the pore walls, indicating the uniform distribution of attapulgite in the sponge.
[0033] Embodiment 4:
[0034] See also Figure 4 This embodiment provides a technical solution based on the second embodiment: Mechanical properties and shape recovery performance test of A / LQC / CS sponge: The mechanical properties of A / LQC / CS sponge were evaluated by cyclic compression test. A cylindrical A / LQC / CS sponge (d×10 mm, h×12 mm) was compressed to 70% strain at a speed of 50 mm / min, and the compression stress-strain curve was obtained to further analyze the compression stress, elasticity and mechanical stability of the sponge.
[0035] The shape recovery performance of A / LQC / CS sponge was evaluated by macro compression test. The initial volume and final volume of A / LQC / CS sponge were recorded as V1 and V2 respectively, and the shape recovery rate of sponge was calculated by the formula. The formula for calculating the shape recovery rate of sponge is as follows: .
[0036] Compared with CS sponge, LQC / CS sponge exhibits lower compressive strength, which is due to the introduction of flexible LQC that destroys the rigid crystal structure of CS. Compared with CS and LQC / CS sponges, A / LQC / CS sponge has significantly improved compressive strength, which is attributed to the introduction of palygorskite. Palygorskite contains a large number of negatively charged silanol groups, which can electrostatically interact with the positively charged quaternary ammonium groups in LQC, thereby enhancing the mechanical strength of the sponge. High mechanical strength enables the hemostatic sponge to maintain its original shape under the compression of injured tissue, providing a long-lasting and effective hemostatic effect. The compressive strength of A / LQC / CS sponge is 84.7±16.6kPa, which is significantly higher than the compressive strength of existing hemostatic sponges, indicating that it has greater advantages in hemostasis.
[0037] In addition, during the cyclic compression process, the A / LQC / CS sponge showed similar stress-strain curves, and the recovery index was close to 1, indicating that it has good elasticity and mechanical stability. The A / LQC / CS sponge can achieve shape fixation under the action of compressive stress. When the compressive stress is released, the shape-fixed A / LQC / CS sponge can spontaneously and quickly restore its initial shape, indicating that it has excellent shape recovery performance, which is attributed to the reversible change of the elastic pore structure inside the A / LQC / CS sponge. The shape recovery time of the hemostatic sponge is positively correlated with its hemostatic ability. Rapid shape recovery is conducive to timely filling and compressing the wound and effectively controlling bleeding. The shape recovery time of the A / LQC / CS sponge is 0.39±0.07s, which is significantly lower than the shape recovery time of the existing hemostatic sponge, indicating that it has greater advantages in hemostasis of non-compressive penetrating injuries.
[0038] Hemostatic materials with good elasticity can evenly distribute pressure on the wound, thereby more effectively slowing or stopping bleeding. This uniform pressure distribution helps to form a stable coagulation environment and promote blood coagulation. Due to the elasticity of the elastic material, it can better adapt to wounds of different shapes and sizes to ensure the hemostatic effect. Whether it is a flat wound or a concave or convex area, the elastic hemostatic material can fit tightly and provide the necessary compression force. Compared with rigid hemostatic materials, elastic hemostatic materials can reduce the patient's sense of pressure and discomfort while providing sufficient compression force. This comfort helps patients better cooperate with treatment and reduce struggling or moving due to pain or discomfort, thereby avoiding further damage to the wound. Appropriate elastic compression can also help promote blood circulation and prevent local ischemia or necrosis caused by long-term compression, which is crucial for wound healing and recovery. When replacing or removing hemostatic materials, elastic materials can reduce friction and pulling on the wound, thereby reducing the risk of secondary injury, which is especially important for patients who need to frequently replace hemostatic materials.
[0039] Embodiment five:
[0040] See also Figure 5 This embodiment provides a technical solution based on the second embodiment: Procoagulant performance test of A / LQC / CS sponge: Gauze, gelatin sponge, CS sponge, LQC / CS sponge or A / LQC / CS sponge (20 mg) were incubated with anticoagulated rabbit whole blood (40 µL) at 37°C for 10 min; 5 ml of deionized water was added to dissolve the exposed and uncoagulated blood cells; the supernatant was collected and the absorbance value of the supernatant at 540 nm was measured using an ELISA reader (A2); the anticoagulated rabbit whole blood that was not incubated with the material was used as the control group, and its absorbance value was recorded as A1; the coagulation index was calculated by the formula, and the formula for calculating the coagulation index is as follows: .
[0041] Gauze, gelatin sponge, CS sponge, LQC / CS sponge or A / LQC / CS sponge (10 mg) were incubated with plasma (1 mL) at 37°C for 10 min. The supernatant was collected and the activated partial thromboplastin time (APTT) and prothrombin time (PT) were measured using an automatic coagulation analyzer. Plasma that was not incubated with the material served as the control group.
[0042] Anticoagulated rabbit whole blood was centrifuged at 3500 rpm for 10 min to obtain red blood cells and platelet-rich plasma; gauze, gelatin sponge, CS sponge, LQC / CS sponge or A / LQC / CS sponge (50 mg) were incubated with blood cells or platelet-rich plasma (0.4 mL) at 37°C for 1 h; the materials were thoroughly washed with normal saline to remove non-adherent red blood cells and platelets; the materials were fixed with 2.5% glutaraldehyde solution for 2 h and then dehydrated with gradient ethanol solution; after freeze-drying, the adhesion, aggregation and activation of red blood cells and platelets on the surface of the materials were observed using scanning electron microscopy.
[0043] The procoagulant properties of A / LQC / CS sponge were evaluated by coagulation index test. The higher the coagulation index, the worse the procoagulant properties. The coagulation index of A / LQC / CS sponge was 42.9±0.4%, which was significantly lower than that of other materials, indicating that it had strong procoagulant ability. Coagulation includes the adhesion, aggregation and activation of blood cells, as well as the activation of intrinsic / exogenous coagulation pathways in the coagulation cascade. Therefore, the procoagulant mechanism of A / LQC / CS sponge was studied by APTT, PT and blood cell adhesion tests; compared with the control group, the APTT and PT values of the A / LQC / CS sponge group were significantly reduced, while the other groups had similar or slightly higher APTT and PT values, indicating that A / LQC / CS sponge was able to activate the endogenous / exogenous coagulation cascade pathways, which was mainly attributed to the introduction of attapulgite. Attapulgite can interact with coagulation factor XII, then self-activate to coagulation factor XIIa, and then activate the endogenous coagulation cascade. It can also activate fibrinogen, reduce coagulation factors in the blood, and shorten the coagulation time. In addition, compared with other materials, more red blood cells and platelets adhered and aggregated on LQC / CS and A / LQC / CS sponges; some deformed platelets were also observed, indicating that they have a strong ability to promote blood cell adhesion, aggregation and activation, which comes from: 1) The porous water-absorbing structure of A / LQC / CS sponge promotes the adhesion and enrichment of blood cells; 2) The hydrophobic alkyl chains and positively charged quaternary ammonium groups not only capture red blood cells and platelets through hydrophobic and electrostatic interactions, but also promote platelet activation; 3) Attapulgite can activate the endogenous / exogenous coagulation pathways and further activate thrombin, which converts fibrinogen into fibrin and promotes the formation of a fibrin network for rapid coagulation.
[0044] Embodiment six:
[0045] See also Figure 6 This embodiment provides a technical solution based on the second embodiment: Hemostatic performance test of A / LQC / CS sponge: Rats were anesthetized by intraperitoneal injection of chloral hydrate, and the liver was exposed after laparotomy. The liver was placed on the surface of filter paper, and a circular penetrating wound with a diameter of 8 mm was created on the liver using a tissue biopsy device. After bleeding, gauze, gelatin sponge, CS sponge, LQC / CS sponge, or A / LQC / CS sponge were filled / injected into the wound cavity to control bleeding. The blood loss was calculated by weighing, and the bleeding time was calculated using a timer.
[0046] New Zealand rabbits were anesthetized by intramuscular injection of sodium pentobarbital. The liver was exposed after laparotomy and placed on the surface of filter paper. A circular penetrating wound with a diameter of 8 mm was created on the liver using a tissue biopsy device. After bleeding, gauze, gelatin sponge, CS sponge, LQC / CS sponge or A / LQC / CS sponge were filled / injected into the wound cavity to control bleeding. The blood loss was calculated by weighing method, and the bleeding time was calculated by timer.
[0047] In the process of non-compression penetrating wound hemostasis, the good shape recovery and procoagulant properties of hemostatic sponges are positively correlated with their hemostatic effects. A / LQC / CS sponges showed excellent shape recovery and procoagulant properties in vitro. In view of this, the in vivo hemostatic properties of A / LQC / CS sponges were evaluated using a rat liver penetrating wound model. Compared with the untreated group, the blood loss and hemostasis time of all treated groups were reduced. Compared with gauze and gelatin sponges, the hemostasis time and blood loss of CS sponges were reduced, which was attributed to the improved shape recovery properties and mechanical strength. Compared with CS sponges, LQC / CS sponges have higher hemostatic properties, which is attributed to the introduction of LQC. LQC enhances the electrostatic and hydrophobic interactions between sponges and blood cells, thereby promoting the adhesion, aggregation and activation of blood cells. A / LQC / CS sponges show better hemostatic ability than LQC / CS sponges, which is attributed to the introduction of attapulgite. Attapulgite enhances the mechanical strength of the sponge, activates the collective endogenous / exogenous coagulation cascade reaction, and accelerates blood solidification. The in vivo hemostatic properties of A / LQC / CS sponge were further evaluated using a New Zealand rabbit liver penetrating injury model. A / LQC / CS sponge exhibited superior hemostatic properties compared with gauze, gelatin sponge, CS sponge, and LQC / CS sponge, which was attributed to the synergistic effects of the porous structure, LQC, and attapulgite.
[0048] The A / LQC / CS sponge injected into the wound cavity can quickly and spontaneously restore its original shape, fill and compress the wound, control bleeding, and reduce blood loss, which is crucial for quickly stabilizing the patient's vital signs in emergency situations (such as trauma, surgery, etc.); materials with good hemostatic effects can timely control bleeding, reduce the risk of serious complications such as hypotension and shock caused by continued bleeding, and ensure the safety of patients.
[0049] Hemostasis is the first step in wound healing. Materials with good hemostatic effects can quickly stop bleeding and provide a clean and dry environment for the wound, which is conducive to further treatment and healing of the wound. Bleeding is often accompanied by pain, and materials with good hemostatic effects can quickly control bleeding, thereby reducing the patient's pain. Reducing bleeding also means reducing the risk of wound irritation and infection, further improving the patient's comfort. In the medical process, hemostasis is a prerequisite for many treatment steps. Materials with good hemostatic effects can quickly complete the hemostasis task, providing convenience for subsequent treatment steps (such as suturing, bandaging, etc.), thereby improving medical efficiency. Timely and effective hemostasis can reduce the consumption of medical resources such as blood transfusions and hospitalization required by patients due to excessive bleeding, thereby reducing medical costs.
[0050] Embodiment seven:
[0051] See also Figure 7 This embodiment provides a technical solution based on the second embodiment: Antibacterial performance test of A / LQC / CS sponge: Gauze, gelatin sponge, CS sponge, LQC / CS sponge and A / LQC / CS sponge were exposed to ultraviolet radiation for 2 hours and then placed in 48-well cell culture plates. Staphylococcus aureus, Escherichia coli or methicillin-resistant Staphylococcus aureus bacterial solution (200 μL, 1×10 6 CFU·mL -1 ); After incubation at 37°C for 2h, transfer the material to 6mL of physiological saline, vortex and oscillate to reselect live bacteria; evenly spread 50μL of resuspended bacterial solution on LB agar medium; after incubation at 37°C for 2h, photograph the colony units of gauze, gelatin sponge, CS sponge, LQC / CS sponge and A / LQC / CS sponge groups; count the number of colony units formed (Y2); LB agar medium was used as the control group, and the number of colony units was recorded as Y1; the sterilization rate of the material was calculated by the formula, and the formula for calculating the sterilization rate of the material is as follows: .
[0052] A large amount of blood loss can cause a decrease in the body's immunity, making the wound susceptible to bacterial infection, leading to serious complications or high mortality (posing a major threat to life). An ideal hemostatic sponge should have efficient antibacterial activity to resist bacterial infection. Alkylation and quaternization polymers have been shown to have broad-spectrum antibacterial properties, which are attributed to their strong hydrophobic and electrostatic interactions with bacterial membranes. Therefore, the plate count method was used to evaluate the antibacterial activity of A / LQC / CS sponge against Staphylococcus aureus and Escherichia coli. Compared with gauze, gelatin sponge and CS sponge groups, LQC / CS sponge had a higher bactericidal rate, which was attributed to the introduction of LQC. LQC contains hydrophobic alkyl chains and positively charged quaternary ammonium groups, which can interact with bacterial membranes, destroy their integrity, and lead to bacterial death. The A / LQC / CS sponge has an antibacterial rate comparable to that of the LQC / CS sponge, indicating that the introduction of attapulgite has no significant effect on the antibacterial activity of the sponge. In clinical practice, excessive use of antibiotics can easily lead to bacterial resistance. Therefore, the plate count method was used to further evaluate the antibacterial activity of A / LQC / CS sponge against methicillin-resistant Staphylococcus aureus. The antibacterial activity of A / LQC / CS sponge against methicillin-resistant Staphylococcus aureus was superior to that of gauze, gelatin sponge and CS sponge, indicating that A / LQC / CS sponge has greater advantages in preventing wound infection.
[0053] Embodiment eight:
[0054] See also Figure 8 , this embodiment provides a technical solution based on the second embodiment: biocompatibility and biosafety of A / LQC / CS sponge.
[0055] The cell compatibility of gauze, gelatin sponge, CS sponge, LQC / CS sponge and A / LQC / CS sponge with NIH 3T3 fibroblasts was evaluated by CCK-8 and live / dead staining. The sterilized materials were immersed in DMEM culture medium and placed at 37°C for 3 days to obtain the extract of the materials. 3T3 fibroblasts were seeded in 96-well plates at a density of 5000 cells per well. After incubation at 37°C overnight, DMEM was aspirated, the cells were washed twice with phosphate buffer solution (PBS, pH=7.4), and then 200μL of the extract was added to each well. After incubation at 37°C for 1, 3 and 5 days, 20μL of CCK-8 reagent was added to each well. After further incubation at 37°C for 2 h, the supernatant was taken and its optical density at 450nm was measured using an enzyme reader. Alternatively, a live / dead staining reagent was added to each well; the cells were incubated at 37°C for 30 min, and the cells were observed and images were acquired using a laser confocal scanning electron microscope.
[0056] The blood compatibility of gauze, gelatin sponge, CS sponge, LQC / CS sponge and A / LQC / CS sponge was evaluated by hemolysis test. Red blood cells were diluted with physiological saline to obtain a solution with a final concentration of 0.2% (v / v); the material (10 mg) was placed in 1 mL of the diluted solution and incubated at 37°C for 30 min; the mixture was centrifuged at 3500 rpm for 10 min to obtain the supernatant; 100 µL of the supernatant was taken and its absorbance at 540 nm was measured using an ELISA reader (A1); the red blood cell solution diluted with water and the red blood cell solution diluted with physiological saline were used as positive and negative controls, respectively, and the corresponding absorbance values were recorded as A2 and A3, respectively; the material hemolysis rate was calculated by the formula, and the formula for calculating the material hemolysis rate is as follows: .
[0057] The tissue compatibility and biosafety of A / LQC / CS sponge were evaluated by subcutaneous implantation test. Gelatin sponge was used as control. Rats were anesthetized by intraperitoneal injection of chloral hydrate, and two incisions were made on both sides of their backs after shaving the hair in the local area of their backs. A round sponge was implanted in each incision, and the incisions were sutured; after feeding for 7 and 28 days, the rats were anesthetized, and the implanted sponges were collected for H&E histological staining and IL-6 immunofluorescence staining to evaluate the inflammatory response of the sponge, that is, histocompatibility. Blood and major organs (heart, liver, spleen, lung and kidney) were collected for blood routine / serum biochemical tests and H&E histological staining to evaluate the biosafety of the sponge.
[0058] The biocompatibility and biosafety of A / LQC / CS sponge are the basic requirements for its application as a hemostatic material or wound dressing. The supernatant of the A / LQC / CS sponge group was light red, and the hemolysis rate was below the acceptable limit of 5%. The A / LQC / CS sponge group had comparable hemolysis rates with other groups, especially the saline, gauze, and gelatin sponge groups, indicating good blood compatibility. As the culture time was extended from 1 d to 5 d, the optical density values of each group gradually increased. Specifically, the optical density values of the A / LQC / CS sponge group were comparable to those of the other groups, and no dead cells were observed, indicating that the A / LQC / CS sponge had good cell compatibility. After 7 d of implantation, the number of inflammatory cells in the A / LQC / CS sponge group increased, and the expression of IL-6 was significantly higher than that in the control group, which was attributed to the acute inflammatory response of the immune system to external substances. After 28 d of implantation, the expression level of IL-6 in the A / LQC / CS sponge group was significantly reduced, comparable to that in the control group, and the inflammatory response was alleviated. In addition, compared with other groups, no pathological changes were observed in the heart, liver, spleen, lung and kidney of the A / LQC / CS sponge group; the A / LQC / CS sponge group had comparable blood routine and serum biochemical index values, indicating good biosafety. The above results collectively indicate that the A / LQC / CS sponge has good biocompatibility.
[0059] Embodiment nine:
[0060] See also Fig. 9 This embodiment provides a technical solution based on the second embodiment: Wound healing performance test of A / LQC / CS sponge: A rat full-thickness skin defect model is used to evaluate the ability of A / LQC / CS sponge to promote wound healing.
[0061] Rats were anesthetized by intraperitoneal injection of chloral hydrate, and their back hair was shaved and the skin was disinfected with iodine. Then, a tissue biopsy device was used to create two circular wounds with a diameter of 1 cm on both sides of the rat's back, and the area was recorded as S1. Then, a circular A / LQC / CS sponge with a diameter of 1 cm or a commercial 3M Tegaderm dressing was covered on each wound. The A / LQC / CS sponge or the commercial 3M Tegaderm dressing was further fixed to the wound position with an elastic bandage to prevent the sponge from falling off and the wound from shrinking naturally. At 7 and 14 days after surgery, the wound surface was photographed, and the wound area (S2) was analyzed using Image-J software. The wound closure rate was calculated by the formula, which is as follows: .
[0062] After hemostasis, wound healing becomes an urgent issue to consider. Porous sponges can absorb excess wound exudate, promote nutrient transport, reduce the risk of infection, and promote cell migration, which have significant advantages in promoting wound healing. In addition, alkylated and quaternized CS have excellent hemostatic, anti-infective and wound healing properties. Therefore, the ability of A / LQC / CS sponge to promote wound healing was evaluated in a rat full-thickness skin defect model. As time went on, the wounds treated with A / LQC / CS sponge and 3M Tegaderm dressing gradually healed; compared with the 3M Tegaderm dressing group, the wound area in the A / LQC / CS sponge group was smaller and the wound closure rate was higher, indicating that the A / LQC / CS sponge has a stronger ability to promote wound healing than the 3M Tegaderm dressing, which may be attributed to the inherent ability of CS to accelerate re-epithelialization and collagen deposition, reduce inflammation and promote angiogenesis.
[0063] The above description is only by way of illustration of certain exemplary embodiments of the present invention. It is undoubted that those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the above drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.
Claims
1. An antibacterial hemostatic material based on chitosan, characterized in that: The antibacterial hemostatic material is an A / LQC / CS sponge, which includes three components: chitosan, lauric acid-modified quaternary ammonium chitosan and attapulgite. The mass ratio of chitosan to lauric acid-modified quaternary ammonium chitosan is 4:
1.
2. A method for preparing an antibacterial hemostatic material based on chitosan, which is applicable to the antibacterial hemostatic material based on chitosan according to claim 1, characterized in that: The following steps are involved: S1, firstly preparing quaternized chitosan; S2, then preparing lauric acid modified quaternary ammonium chitosan; S3. Finally, prepare A / LQC / CS sponge.
3. The method for preparing an antibacterial hemostatic material based on chitosan according to claim 2, characterized in that: The preparation of the quaternized chitosan described in S1 comprises the following steps: S11, dispersing chitosan in deionized water, adding glacial acetic acid and stirring to obtain a chitosan solution; S12, dissolving 2,3-epoxypropyltrimethylammonium chloride in deionized water, adding the 2,3-epoxypropyltrimethylammonium chloride solution dropwise into the chitosan solution for reaction, placing the reaction solution into a dialysis bag, dialyzing it in deionized water, and freeze-drying it to obtain quaternized chitosan.
4. The method for preparing an antibacterial hemostatic material based on chitosan according to claim 2, characterized in that: The preparation of the lauric acid modified quaternary ammonium chitosan described in S2 comprises the following steps: S21, dissolving quaternized chitosan in deionized water, dissolving carbodiimide hydrochloride, N-hydroxysuccinimide and lauric acid in methanol for activation, adding QCS solution dropwise to the activation solution, and reacting at room temperature; S22, putting the reaction solution into a dialysis bag, dialyzing it in deionized water, and freeze-drying it to obtain lauric acid-modified quaternary ammonium chitosan.
5. The method for preparing an antibacterial hemostatic material based on chitosan according to claim 2, characterized in that: The preparation of the A / LQC / CS sponge described in S3 comprises the following steps: S31, firstly preparing LQC / CS sponge; S32. Finally, prepare A / LQC / CS sponge.
6. The method for preparing an antibacterial hemostatic material based on chitosan according to claim 5, characterized in that: The preparation of the LQC / CS sponge described in S31 comprises the following steps: Chitosan and lauric acid-modified quaternized chitosan were dissolved in an acetic acid aqueous solution to obtain a composite solution, which was then centrifuged and poured into a mold, and finally freeze-dried to obtain an LQC / CS sponge.
7. The method for preparing an antibacterial hemostatic material based on chitosan according to claim 5, characterized in that: The preparation of the A / LQC / CS sponge described in S32 comprises the following steps: The LQC / CS sponge was soaked in an ethanol / sodium hydroxide solution and then washed with water. After washing, the LQC / CS sponge was compressed and placed in a attapulgite suspension to obtain an LQC / CS sponge loaded with attapulgite, namely, A / LQC / CS sponge.
8. The method for preparing an antibacterial hemostatic material based on chitosan according to claim 7, characterized in that: The mass volume percentage of attapulgite in the attapulgite suspension is 3%.
9. Use of the chitosan-based antibacterial hemostatic material according to claim 1 in the preparation of a medical hemostatic sponge.
10. Use of the chitosan-based antibacterial hemostatic material prepared by the preparation method according to any one of claims 2 to 8 in the preparation of a medical hemostatic sponge.
Citation Information
Patent Citations
Nano-silver antibacterial sanitary towel and production method thereof
CN107456321A
Composite sponge as well as preparation method and application thereof
CN111870731A
Collagen hydrogel as well as preparation method and application thereof
CN116510070A
Cationic amphiphilic chitosan quaternary ammonium salt as well as preparation method and application thereof
CN117659225A
Chitosan / quaternized chitosan sponge as well as preparation method and application thereof
CN118001450A
Cited By
Active oxygen responsive hydrogen sulfide donor, active oxygen responsive hydrogen sulfide controllable release type cationized chitosan sponge, preparation method and application
CN121248644A
An active oxygen responsive hydrogen sulfide donor, an active oxygen responsive hydrogen sulfide controllable release type cationized chitosan sponge, a preparation method and application thereof
CN121248644B
