Multilayer hernia repair patch as well as preparation method and application thereof
By using a multi-layer structure of polymer fabric layer, micro-nano film layer and antimicrobial peptide layer in the hernia repair patch, the problems of insufficient biocompatibility and antibacterial properties of the existing hernia repair patch are solved, and efficient antimicrobial peptide relief is achieved. The release and mechanical properties are improved, making it suitable for use as an anti-infective patch.
Patent Information
- Application Number
- CN202410827538.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-22
AI Technical Summary
Existing hernia repair patches have deficiencies in biocompatibility, antibacterial and anti-inflammatory effects, and mechanical properties, resulting in a high risk of implant-related infection.
It adopts a multi-layer hernia repair patch structure, including a polymer fabric layer, a micro-nano film layer and an antimicrobial peptide layer. It is connected through an intermediate layer and uses antimicrobial peptides for sustained release to improve biocompatibility and antibacterial properties.
It has achieved good biocompatibility, mechanical properties and significant antibacterial effect, and the sustained release performance of antibacterial peptides has been significantly improved. It is suitable for industrial production and has broad application potential for anti-infective patches.
Smart Images

Figure CN118806987A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medical materials, and in particular relates to a multi-layer hernia repair sheet and a preparation method and application thereof. Background Art
[0002] Implant-associated infection is a serious surgical complication, and it is reported that about 5% of hernia repair surgeries will have infectious complications. More than 1 million people in the United States suffer from hernias each year, and nearly 14% of people in the United Kingdom suffer from hernias each year. Therefore, considering the large number of cases each year, the number of infections cannot be underestimated. Infection during hernia repair is a surgical disaster for patients, causing severe pain and huge costs. Bacterial infection is the main cause of the above infections. The most common bacteria in the infections are Staphylococcus aureus (SA), Staphylococcus epidermidis, Escherichia coli (EC), Pseudomonas aeruginosa (PA), Proteus and Streptococcus pyogenes.
[0003] Tension-free hernia repair surgery uses a patch to repair the hernia gap, avoiding the shortcomings of traditional hernia repair surgery, such as postoperative pain and easy recurrence. Currently, the commonly used hernia repair patches are polyester patches, polypropylene substrates, and expanded polytetrafluoroethylene patches. In the past 50 years, polypropylene substrates have had a huge impact on the field of surgery, and it has been proven to be the most popular implant in the field of surgery today. Despite this, there are also some problems with polypropylene substrates in their application, such as poor biocompatibility, unstable antibacterial and anti-inflammatory effects, easy stratification, and poor mechanical properties. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a multi-layer hernia repair patch, which has good biocompatibility, sufficient mechanical properties and obvious antibacterial properties, and the antimicrobial peptide shows a good sustained release effect.
[0005] The invention also provides a method for preparing the multi-layer hernia repair sheet.
[0006] The present invention also provides an application.
[0007] According to a first aspect of the present invention, a multilayer hernia repair patch is provided, comprising a polymer fabric layer, on which a micro-nano film layer and an antimicrobial peptide layer are arranged, and the polymer fabric layer and the micro-nano film layer are connected by an intermediate layer.
[0008] In some embodiments of the present invention, the polymer fabric layer includes a fabric formed of at least one of polypropylene, polylactic acid, nylon, polyvinylidene fluoride, polyester, and polytetrafluoroethylene.
[0009] In some preferred embodiments of the present invention, the polymer fabric layer is a fabric formed of polypropylene.
[0010] In some preferred embodiments of the present invention, the fabric comprises a fabric formed by weaving, knitting or braiding in the form of monofilaments and / or multifilaments.
[0011] In some more preferred embodiments of the present invention, the knitting includes warp knitting and weft knitting.
[0012] In some embodiments of the present invention, the raw material of the micro-nano film layer includes at least one of polycaprolactone, polylactic acid, collagen, gelatin, chitosan and polylactic acid-glycolic acid copolymer.
[0013] In some preferred embodiments of the present invention, the raw material of the micro-nano film layer is polycaprolactone.
[0014] In some embodiments of the present invention, the raw materials of the antimicrobial peptide layer include cationic polypeptides and polysaccharides.
[0015] In some preferred embodiments of the present invention, the polysaccharide includes at least one of gellan gum, xanthan gum, gelatin, chitosan, chitosan derivatives, alginate, carboxymethyl cellulose salt, hyaluronate and hyaluronic acid derivatives.
[0016] In some embodiments of the present invention, the raw material of the middle layer includes polysaccharide.
[0017] In some preferred embodiments of the present invention, the polysaccharide includes at least one of gellan gum, xanthan gum, gelatin, chitosan, chitosan derivatives, alginate, carboxymethyl cellulose salt, hyaluronate and hyaluronic acid derivatives.
[0018] In some more preferred embodiments of the present invention, the polysaccharide is gellan gum.
[0019] In some embodiments of the present invention, the content of antimicrobial peptide in the antimicrobial peptide layer is 1-10 mg / cm 2 .
[0020] In some embodiments of the present invention, the polysaccharide content in the intermediate layer is 1 to 3 mg / cm 2 .
[0021] In some preferred embodiments of the present invention, the polysaccharide content in the intermediate layer is 2 mg / cm 2 .
[0022] In some embodiments of the present invention, the content of the high molecular weight polymer in the micro-nano film layer is 0.5-2 mg / cm 2 .
[0023] In some preferred embodiments of the present invention, the polymer content in the micro-nano film layer is 0.75 mg / cm 2 .
[0024] According to a second aspect of the present invention, a method for preparing the multilayer hernia repair sheet according to the first aspect of the present invention is provided, the preparation method comprising the following steps:
[0025] S1: covering a layer of polysaccharide solution on the polymer fabric layer to obtain a substrate covered with an intermediate layer;
[0026] S2: using the substrate covered with the intermediate layer in step S1 as a receiving device, taking the spinning solution for spinning to obtain a substrate covered with a micro-nano film layer;
[0027] S3: Covering a layer of polysaccharide solution on the substrate covered with the micro-nano film layer in step S2, and then spraying a layer of antimicrobial peptide solution to obtain a multi-layer hernia repair sheet.
[0028] In some embodiments of the present invention, the polymer fabric layer in step S1 includes a fabric formed of at least one of polypropylene, polylactic acid, nylon, polyvinylidene fluoride, polyester and polytetrafluoroethylene.
[0029] In some preferred embodiments of the present invention, the polymer fabric layer is a fabric formed of polypropylene.
[0030] In some preferred embodiments of the present invention, the fabric comprises a fabric formed by weaving, knitting or braiding in the form of monofilaments and / or multifilaments.
[0031] In some more preferred embodiments of the present invention, the knitting includes warp knitting and weft knitting.
[0032] In some embodiments of the present invention, the polysaccharide solution in step S1 and step S3 includes a solution of at least one of gellan gum, xanthan gum, gelatin, chitosan, chitosan derivatives, alginate, carboxymethyl cellulose salt, hyaluronate and hyaluronic acid derivatives.
[0033] In some preferred embodiments of the present invention, the polysaccharide solution is a gellan gum solution.
[0034] In some preferred embodiments of the present invention, the concentration of the polysaccharide solution is 1-100 g / L.
[0035] In some more preferred embodiments of the present invention, the concentration of the polysaccharide solution is 5 to 20 g / L.
[0036] In some more preferred embodiments of the present invention, the concentration of the polysaccharide solution is 8 g / L.
[0037] In some embodiments of the present invention, the polysaccharide solution is sterilized before covering.
[0038] In some preferred embodiments of the present invention, the sterilization temperature is 100-150°C.
[0039] In some more preferred embodiments of the present invention, the sterilization temperature is 120°C.
[0040] In some preferred embodiments of the present invention, the disinfection time is 20 to 40 minutes.
[0041] In some more preferred embodiments of the present invention, the disinfection time is 30 minutes.
[0042] In some preferred embodiments of the present invention, the sterilization pressure is 0-30 MPa.
[0043] In some embodiments of the present invention, the spinning solution in step S2 contains 50-200 g / L of high molecular polymer.
[0044] In some preferred embodiments of the present invention, the spinning solution in step S2 contains 80-150 g / L of high molecular weight polymer.
[0045] In some more preferred embodiments of the present invention, the spinning solution in step S2 contains 100 g / L of high molecular weight polymer.
[0046] In some preferred embodiments of the present invention, the high molecular polymer includes at least one of polycaprolactone, polylactic acid, collagen, gelatin, chitosan and polylactic acid-glycolic acid copolymer.
[0047] In some more preferred embodiments of the present invention, the polymer is polycaprolactone.
[0048] In some preferred embodiments of the present invention, the solvent of the spinning solution includes at least one of hexafluoroisopropanol, dichloromethane, N,N-dimethylformamide, tetrahydrofuran, chloroform, acetic acid and water.
[0049] In some embodiments of the present invention, the receiving device in step S2 is placed on aluminum foil during spinning.
[0050] In some embodiments of the present invention, the spinning in step S2 includes electrospinning.
[0051] In some preferred embodiments of the present invention, the voltage of the electrospinning is 10-20 kV.
[0052] In some more preferred embodiments of the present invention, the voltage of the electrospinning is 13 kV.
[0053] In some preferred embodiments of the present invention, the receiving distance of the electrospinning is 10 to 20 cm.
[0054] In some more preferred embodiments of the present invention, the receiving distance of the electrospinning is 15 cm.
[0055] In some preferred embodiments of the present invention, the electrospinning solution advancing speed is 1 to 2 mL / h.
[0056] In some more preferred embodiments of the present invention, the electrospinning solution advancing speed is 1.5 mL / h.
[0057] In some embodiments of the present invention, the antimicrobial peptide solution in step S3 contains 0.01-50 g / L antimicrobial peptide.
[0058] In some preferred embodiments of the present invention, the antimicrobial peptide comprises a cationic polypeptide.
[0059] In some more preferred embodiments of the present invention, the antimicrobial peptide comprises a polypeptide having an amino acid sequence as shown in SEQ ID NO:1.
[0060] In some preferred embodiments of the present invention, the antimicrobial peptide solution is filtered and sterilized before spraying.
[0061] In some more preferred embodiments of the present invention, the filtration sterilization uses a 0.2 μm filter membrane.
[0062] According to a third aspect of the present invention, a use of the multilayer hernia repair sheet as described in the first aspect of the present invention in preparing a product for treating hernia is proposed.
[0063] The present invention has at least the following beneficial effects:
[0064] Based on the antibacterial mechanism of antibacterial peptides that is different from traditional antibiotics, the present invention proposes a multi-layer hernia patch and its preparation method and application, the multi-layer hernia patch includes a polymer fabric layer, a micro-nano film layer, an antibacterial peptide layer and an intermediate layer are arranged on the polymer fabric layer, and the multi-layer patch finally obtained has good biocompatibility, sufficient mechanical properties and obvious antibacterial properties, and the peptides show good sustained-release effect. The preparation method of the multi-layer hernia patch is simple in steps and suitable for industrial production. The multi-layer patch has the potential to be widely used as an anti-infection patch. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:
[0066] Figure 1 A schematic diagram of the structure of a multi-layer hernia repair patch provided in Example 1 of the present invention;
[0067] Figure 2 This is a graph showing the test results of the in vitro sustained-release performance of the antibacterial polypeptide in the test example of the present invention from 0 to 240 hours;
[0068] Figure 3 This is a graph showing the test results of the in vitro sustained-release performance of the antibacterial polypeptide in the test example of the present invention at 0 to 24 hours;
[0069] Figure 4 The figures are the test results of mechanical properties of each group of patches in the test examples of the present invention; wherein (a) is the tensile breaking strength result figure, and (b) is the elastic modulus result figure; "Warp" refers to the sample cut in the warp direction, "Weft" refers to the sample cut in the weft direction, "PP" refers to the polypropylene patch, and "A" refers to the patch provided in Example 1; different lowercase letters marked in the figures represent significant differences between the groups;
[0070] Figure 5 The graph is a test result of the antibacterial performance of the patch in the test example of the present invention; wherein A to D represent the patches provided in Examples 1 to 4 respectively;
[0071] Figure 6 The in vitro cytotoxicity test results of the patches in the test examples of the present invention are shown in the figure; wherein A to D represent the patches provided in Examples 1 to 4, respectively; different lowercase letters marked in the figure represent significant differences between the groups. DETAILED DESCRIPTION
[0072] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0073] Example 1
[0074] This embodiment provides a multi-layer hernia repair patch, and the preparation method of the multi-layer hernia repair patch specifically includes the following steps:
[0075] 1) Preparation of polysaccharide solution:
[0076] Weigh 0.8 g of gellan gum powder and dissolve it in 100 mL of deionized water, sterilize it at 120° C. and 103 kPa for 30 minutes, and cool it to obtain a 0.8% (w / v) polysaccharide solution for use;
[0077] 2) Preparation of spinning solution:
[0078] Weigh 10 g of polycaprolactone particles, add 100 mL of hexafluoroisopropanol solution thereto, and stir magnetically for 24 h until the solution becomes transparent and uniform, to obtain a 10% (w / v) polycaprolactone spinning solution;
[0079] 3) Prepare the electrospinning receiving device:
[0080] Take a warp knitted macroporous polypropylene patch (pore size 3.5mm×3.06mm, porosity of about 73.35, surface density of about 46.78g / m 2 , the patch thickness is about 0.56mm) as the substrate, put it on the aluminum foil, and spread a layer of the polysaccharide solution obtained in step 1) on the polypropylene patch to obtain a polypropylene patch covered with an intermediate layer (the content of polysaccharide in the patch is 2mg / cm 2 ), which is used as an electrospinning receiving device;
[0081] 4) Perform electrospinning:
[0082] The spinning solution obtained in step 2) is used to perform electrospinning on the middle layer of the receiving device obtained in step 3), the high voltage used is 13 kV, the receiving distance is 15 cm, and the propulsion speed of the spinning solution is 25 μL / min, to obtain a polycaprolactone / polypropylene composite patch;
[0083] 5) Preparation of antimicrobial peptide solution:
[0084] The polypeptide was dissolved in deionized water, filtered and sterilized with a 0.2 μm filter to obtain an antimicrobial peptide stock solution with a final concentration of 50 mg / mL, which was diluted to 5 mg / mL with deionized water when used; the above polypeptide was a cationic polypeptide PEP-1 synthesized in the laboratory, and the amino acid sequence of PEP-1 was RRRGRRRGPPGRRRGRRR (SEQ ID NO: 1).
[0085] 6) The polycaprolactone / polypropylene composite patch obtained in step 4) was irradiated with ultraviolet light on both sides for 1 hour for disinfection, and a layer of polysaccharide solution obtained in step 1) was coated on the polycaprolactone electrospun layer (micro-nano film layer), that is, a layer of polysaccharide was covered on the polycaprolactone electrospun layer (the content of polysaccharide in the patch was 2 mg / cm at this time). 2 ); spray the 5 mg / mL antimicrobial peptide solution obtained in step 5) evenly on the polysaccharide to make each square centimeter of the patch contain 1 mg of antimicrobial peptide, dry naturally, and obtain a multi-layer hernia repair patch, which is packaged in a sterile bag for standby use; the structure of the multi-layer hernia repair patch is as follows Figure 1 shown.
[0086] Example 2
[0087] This embodiment provides a multi-layer hernia repair patch. The preparation method of the multi-layer hernia repair patch is different from that of Example 1 only in that the concentration of the antimicrobial peptide solution obtained in step 5) is adjusted to 15 mg / mL, so that the final multi-layer hernia repair patch contains 3 mg of antimicrobial peptide per square centimeter, and the remaining steps are the same.
[0088] Example 3
[0089] This embodiment provides a multi-layer hernia repair patch. The preparation method of the multi-layer hernia repair patch is different from that of Example 1 only in that the concentration of the antimicrobial peptide solution obtained in step 5) is adjusted to 25 mg / mL, so that the final multi-layer hernia repair patch contains 5 mg of antimicrobial peptide per square centimeter, and the remaining steps are the same.
[0090] Example 4
[0091] This embodiment provides a multi-layer hernia repair patch. The preparation method of the multi-layer hernia repair patch is different from that of Example 1 only in that the concentration of the antimicrobial peptide solution obtained in step 5) is adjusted to 50 mg / mL, so that the final multi-layer hernia repair patch contains 10 mg of antimicrobial peptide per square centimeter, and the remaining steps are the same.
[0092] Comparative Example 1
[0093] This comparative example uses the commercially available patch product PROCEED (article number PCDG1) from Johnson & Johnson of the United States.
[0094] Comparative Example 2
[0095] This comparative example uses the commercially available patch product Prolene (article number PMII) from Johnson & Johnson of the United States.
[0096] Comparative Example 3
[0097] This comparative example uses the commercially available patch product Prolene soft (article number SPMH) from Johnson & Johnson of the United States.
[0098] Test example
[0099] This test example tests the performance of the patches provided by Examples 1 to 4 and Comparative Examples 1 to 3, specifically including the test of the in vitro release rate, mechanical properties, antibacterial ability and cytotoxicity of the multilayer hernia patch. The test steps and test results are as follows:
[0100] 1. In vitro release characteristics test of antimicrobial peptides:
[0101] This test example tests the antimicrobial peptide release rate of the multilayer hernia repair patch provided in Example 1 in an in vitro environment, and the specific steps are as follows:
[0102] 1) The multilayer hernia repair patch sample (10×10 mm) prepared in Example 1 was placed in 1 mL of PBS, placed on a shaker, and shaken at 100 r / min at 37° C.; samples were taken once at 2 h, 4 h, 6 h, and 24 h after the start of the test, and then once a day for a total of 10 days, 100 μL of supernatant was taken out each time, and 100 μL of fresh PBS was added;
[0103] 2) Using NanoDrop TM 2000 Ultra-micro Spectrophotometer (Thermo Scientific TM , USA) to measure the absorbance value; since tryptophan exhibits a strong UV-vis signal at 280nm, in order to more accurately detect the concentration of the antibacterial polypeptide in the sample, the two arginine residues (the arginine residues at the first position and the second position) in the polypeptide sequence described in Example 1 were replaced by tryptophan residues for testing;
[0104] 3) Calculate the peptide concentration based on the standard curve generated by the absorbance values of different peptide concentrations at 280nm; this experiment was carried out 3 times, and 10 absorbance values were measured at each time point; the results are as follows Figure 2 and Figure 3 shown.
[0105] Depend on Figure 2 and Figure 3 It can be seen that after 6 hours of culture, about 15.1% of the antimicrobial peptides were released, and less than 60% of the antimicrobial peptides were released within 10 days. It can be seen that the multi-layer hernia repair patch provided by the present invention can slowly release the antimicrobial peptide components therein over a relatively long period of time, and the multi-layer hernia repair patch has good sustained-release performance.
[0106] 2. Mechanical properties test:
[0107] This test example tests the mechanical properties of the patches provided in Example 1 and Comparative Examples 1 to 3, and the specific steps are as follows:
[0108] 1) Warp knitted fabrics generally have anisotropy. This test example uses the polypropylene patch described in step 3) of Example 1 as a control group for testing;
[0109] 2) Cut the patches provided in Example 1 and Comparative Examples 1 to 3 into samples of 1×4.5 cm in size along the radial and latitudinal directions of the patches;
[0110] 3) Use a Japanese Shimadzu EZ Graph tensile tester and Trapezium 2.32 data acquisition software; set the stretching speed to 25 mm / min and the stretching distance to 15 mm; collect the maximum tensile stress at break and the elastic modulus in the linear stretching stage; repeat each test 5 times. Calculate the average and standard deviation, and the results are as follows: Figure 4 shown.
[0111] Depend on Figure 4 It can be seen that there is no significant difference between the multilayer hernia repair patch (sample A) provided in Example 1 and the existing commercial patch PROLENE Soft, indicating that its mechanical properties meet the requirements.
[0112] 3. Antibacterial performance test:
[0113] This test example tests the antibacterial properties of the multilayer hernia repair sheets provided in Examples 1 to 4, and the specific steps are as follows:
[0114] The antibacterial properties of the patches provided in Examples 1 to 4 were tested using the inhibition zone method; each group of samples was cut into 1×1 cm pieces (4 pieces per group of samples) under sterile conditions;
[0115] The density of Escherichia coli was adjusted to 3 × 10 6 CFU / mL (1~5×10 6 CFU / mL), evenly spread 100 μL of bacterial solution on LB agar plate; then carefully place the sample on the agar plate, incubate at 37°C for 24 hours, and then observe and measure the diameter of the inhibition zone; the results are as follows Figure 5 As shown; wherein, A to D represent embodiments 1 to 4 respectively.
[0116] Depend on Figure 5 It can be seen that the multilayer hernia repair sheets provided in Examples 1 to 4 all showed significant inhibitory effects on Escherichia coli, and as the concentration of the antibacterial polypeptide increased, the inhibition zone value increased and the antibacterial effect was enhanced.
[0117] 4. Cytotoxicity test:
[0118] This test example tests the cytotoxicity of the extracts of the multilayer hernia repair sheets provided in Examples 1 to 4 to human dermal fibroblasts (HDFs) according to the fifth part of the in vitro cytotoxicity test standard of the international standard ISO 10993-5-2009. The specific steps are as follows:
[0119] 1) 10% DMSO solution was used as negative control (DMSO group), and the extract of the composite patch without polypeptide (the only difference from the patch provided in Example 1 was that no polypeptide was added) was used as positive control (Control);
[0120] 2) Each group of samples was cut into 1×1 cm pieces under sterile conditions and placed in complete culture medium. The ratio of sample surface area to extract volume was 1 cm 2 / mL, incubate in a 37°C, 5% CO2 incubator for 24 h, collect the supernatant to obtain the leaching solution;
[0121] 3) When the second generation HDFs have grown to the bottom of the culture flask, the cells were digested with trypsin-EDTA solution, resuspended by centrifugation, and the cells were counted; 1.5×10 cells were planted in each well of a 48-well culture plate. 4 24 h after inoculation, the original culture medium was replaced with an equal volume of the patch extract obtained in step 2) or the negative control solution (n=5);
[0122] 4) In order to evaluate the activity of each group of sample cells, after 24 hours of the medium replacement treatment in step 3), 20 μL of Alamar Blue (purchased from Bio-RAD) was added to each well, and after 4 hours of incubation in the dark, the fluorescence value was tested using an ELISA reader; 200 μL of complete cell culture medium and 20 μL of Alamar Blue mixture was set as the blank control (Blank group); the results are shown in the figure below. Figure 6 shown.
[0123] Depend on Figure 6 It can be seen that the average fluorescence values of the cells in each group treated with the patches obtained in Examples 1 to 4 have no significant difference with those in the control group, indicating that the multilayer hernia repair patch provided by the present invention has no cytotoxicity to HDFs and has good biocompatibility.
[0124] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A multi-layer hernia repair patch, characterized in that: The multi-layer hernia repair sheet comprises a polymer fabric layer, on which a micro-nano film layer and an antimicrobial peptide layer are arranged, and the polymer fabric layer and the micro-nano film layer are connected by an intermediate layer.
2. The multilayer hernia repair patch according to claim 1, characterized in that: The polymer fabric layer includes a fabric formed of at least one of polypropylene, polylactic acid, nylon, polyvinylidene fluoride, polyester and polytetrafluoroethylene; Preferably, the fabric comprises a fabric formed by weaving, knitting or braiding in the form of monofilament or / and multifilament; More preferably, the knitting includes warp knitting and weft knitting.
3. The multilayer hernia repair patch according to claim 1, characterized in that: The raw material of the micro-nano film layer includes at least one of polycaprolactone, polylactic acid, collagen, gelatin, chitosan and polylactic acid-glycolic acid copolymer.
4. The multilayer hernia repair patch according to claim 1, characterized in that: The raw materials of the antimicrobial peptide layer include cationic polypeptides and polysaccharides; And / or, the raw material of the middle layer includes polysaccharide.
5. The method for preparing the multilayer hernia repair sheet according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: S1: covering a layer of polysaccharide solution on the polymer fabric layer to obtain a substrate covered with an intermediate layer; S2: using the substrate covered with the intermediate layer in step S1 as a receiving device, taking the spinning solution for spinning to obtain a substrate covered with a micro-nano film layer; S3: Covering a layer of polysaccharide solution on the substrate covered with the micro-nano film layer in step S2, and then spraying a layer of antimicrobial peptide solution to obtain a multi-layer hernia repair sheet.
6. The preparation method according to claim 5, characterized in that: The polysaccharide solution in step S1 and step S3 includes a solution of at least one of gellan gum, xanthan gum, gelatin, chitosan, chitosan derivatives, alginate, carboxymethyl cellulose salt, hyaluronate and hyaluronic acid derivatives; Preferably, the concentration of the polysaccharide solution is 1-100 g / L.
7. The preparation method according to claim 5, characterized in that: The spinning solution in step S2 contains 50-200 g / L of high molecular polymer; Preferably, the high molecular polymer includes at least one of polycaprolactone, polylactic acid, collagen, gelatin, chitosan and polylactic acid-glycolic acid copolymer; Preferably, the solvent of the spinning solution includes at least one of hexafluoroisopropanol, dichloromethane, N,N-dimethylformamide, tetrahydrofuran, chloroform, acetic acid and water.
8. The preparation method according to claim 5, characterized in that: The spinning in step S2 includes electrospinning; Preferably, the voltage of the electrospinning is 10 to 20 kV; Preferably, the receiving distance of the electrospinning is 10 to 20 cm; Preferably, the electrospinning solution advancing speed is 1 to 2 mL / h.
9. The preparation method according to claim 5, characterized in that: The antimicrobial peptide solution in step S3 contains 0.01-50 g / L antimicrobial peptide; Preferably, the antimicrobial peptide comprises at least one of arginine, lysine and histidine.
10. Use of the multilayer hernia repair sheet as claimed in any one of claims 1 to 4 in the preparation of a product for treating hernia.