Device and method for preparing nano material through pulse laser induction under liquid phase condition

By designing a pulse laser induction device under liquid phase conditions and utilizing the interaction between laser and solution, the pollution, high cost and complex process problems of nanomaterial preparation in the existing technology have been solved, and efficient, accurate and automated batch production of nanomaterials has been achieved. preparation.

CN118807650APending Publication Date: 2024-10-22NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310478274.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The existing technology lacks devices and methods that can produce nanomaterials in batches or modified batches through pulse laser induction under liquid phase conditions. Traditional preparation methods have problems such as high pollution, complex processes, and high costs.

Method used

A device for the preparation of nanomaterials induced by pulse laser under liquid phase conditions is designed, including a continuous dropping unit, a laser, a convex lens and a concave lens. Through computer control of the pump and solenoid valve, the interaction between the pulse laser and the solution is realized, and the efficient preparation or Modify the nanomaterial, and fill the first container with an inert gas to prevent oxidation.

Benefits of technology

It achieves safe, controllable and effective continuous batch preparation of nanomaterials, improves preparation efficiency, simplifies steps, and uses parallel lasers to optimize the nanomaterial synthesis process to ensure high precision and automation of preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807650A_ABST
    Figure CN118807650A_ABST
Patent Text Reader

Abstract

The invention provides a device and a method for preparing a nano material under liquid phase condition through pulse laser induction, and belongs to the technical field of nano material synthesis, the device comprises a continuous dripping unit, the continuous dripping unit comprises a first container and a second container, an outlet of the first container is provided with a dropper, and the second container is provided with a second dropper; the second container is located below the dropper, and an electromagnetic valve used for controlling the flow rate of liquid in the dropper is arranged between an outlet of the first container and the dropper; the laser device generates laser light in a working state and the laser light is emitted to the dropper; the method has the beneficial effects that a safe, controllable and effective continuous batch nano material preparation technology is provided, batch preparation or modified batch preparation of nano materials can be realized, the preparation efficiency is improved, and the preparation steps are simplified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano material synthesis, and relates to a device and method for preparing nano material by pulse laser induction under liquid phase conditions. Background Art

[0002] Nanomaterials are widely used, and the scale of the Chinese market is constantly expanding. Nanotechnology is the most active research direction in the world's cutting-edge science and technology. Nanotechnology is increasingly used in the diagnosis, treatment, and detection of diseases. Compared with traditional materials, nanomaterials have broad application prospects in the field of medical devices due to their superior nano-effects. In recent years, a series of nanomaterials have been applied to tumor diagnosis and treatment research, but if they are to be transformed, nanomaterials need to consider the characteristics of effectiveness, safety, batch preparation, and low cost. Most traditional preparation methods have high pollution, complex processes, and high batch costs. Therefore, there is an urgent need for an advanced continuous batch preparation technology for nanomaterials that is safe, controllable, and effective.

[0003] The preparation of nanomaterials under liquid phase conditions using pulsed lasers has attracted the attention of many scholars as a green, low-cost and easy-to-operate method. This method mainly utilizes the interaction between lasers and solutions and media to produce local non-equilibrium processes. Through the process of energy concentration and differentiation, it can efficiently and quickly prepare or modify new nanomaterials.

[0004] Currently, there is a lack of equipment that can batch prepare or modify nanomaterials under liquid phase conditions by pulsed laser induction. Summary of the invention

[0005] The purpose of the present invention is to address the above-mentioned problems existing in the prior art and to propose a device and method for preparing nanomaterials by pulsed laser induction under liquid phase conditions.

[0006] The object of the present invention can be achieved by the following technical scheme: A device for preparing nanomaterials by pulsed laser induction under liquid phase conditions, comprising:

[0007] A continuous dripping unit, comprising a first container and a second container, wherein the outlet of the first container is provided with a dripping tube, the second container is located below the dripping tube, and an electromagnetic valve for controlling the flow rate of the liquid in the dripping tube is provided between the outlet of the first container and the dripping tube;

[0008] A laser generates laser light in a working state and irradiates the laser light toward the dropper.

[0009] Preferably, it also includes a convex lens and a concave lens, wherein the convex lens and the concave lens are located on the path of the laser generated by the laser and are arranged in sequence along the emission direction of the laser; in a working state, the pulsed laser emitted by the laser induces the liquid dripping in the dropper after being contracted by the convex lens and the concave lens.

[0010] Preferably, it further comprises a gas cylinder for filling the first container with an inert gas, wherein the gas cylinder is connected to the first container via a gas pipe.

[0011] Preferably, the method further comprises a raw material supply unit for injecting a solution containing nano material powder into the first container, and the raw material supply unit is connected to the first container.

[0012] Preferably, the raw material supply unit includes a mixing bottle and at least two reagent bottles, the reagent bottle is connected to the mixing bottle via a first pipeline, the mixing bottle is connected to the first container via a second pipeline, the first pipeline is provided with a first pump, and the second pipeline is provided with a second pump.

[0013] Preferably, the raw material supply unit further comprises a stirrer, and the mixing bottle is arranged on the stirrer; in a working state, the stirrer stirs the solution in the mixing bottle.

[0014] Preferably, it further comprises a liquid collecting bottle, wherein the liquid collecting bottle is connected to the second container via a third pipeline, and the third pipeline is provided with a third pump.

[0015] Preferably, it also includes a driving unit, a control unit and a computer, the control unit is electrically connected to the computer, the laser is electrically connected to the control unit, the driving unit is electrically connected to the control unit, and the first pump, the second pump, the third pump and the solenoid valve are all electrically connected to the driving unit; in a working state, the computer sends a pulse signal to the laser through the control unit, and at the same time sends a control signal to the driving unit through the control unit to control the switch and flow rate of the first pump, the second pump, the third pump and the solenoid valve.

[0016] A method for preparing nanomaterials by pulsed laser induction under liquid phase conditions is also proposed, comprising the device for preparing nanomaterials by pulsed laser induction under liquid phase conditions, and further comprising the following steps:

[0017] S1: A solution containing nanomaterial powder and a reaction reagent are respectively placed in two reagent bottles, a computer drives a first pump through a control unit and a drive unit to pump the solution in the reagent bottle into a mixing bottle at a set flow rate, and a stirrer stirs the solution in the mixing bottle;

[0018] S2: The computer drives the second pump through the control unit and the driving unit to pump the mixed solution in the mixing bottle into the first container at a set flow rate;

[0019] S3: The computer turns on the laser through the control unit, and the laser emits a pulsed laser toward the dropper. The computer turns on the solenoid valve through the control unit and the drive unit and controls the flow rate of the solution flowing out of the first container. The solution in the first container drips through the dropper to the second container at the set flow rate. The solution dripping from the dropper is induced by the pulsed laser, and the product induced by the pulsed laser falls into the second container.

[0020] S4: The computer drives the third pump through the control unit and the driving unit to pump the product solution in the second container into the liquid collection bottle at a set flow rate.

[0021] Preferably, in step S2, if there is a need for an inert gas environment in the first container during the preparation process, the gas cylinder is opened and the inert gas in the gas cylinder enters into the first container.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. A safe, controllable and effective continuous batch preparation technology for nanomaterials is proposed, which can be used for batch preparation or modified batch preparation of nanomaterials, which not only improves the preparation efficiency but also simplifies the preparation steps.

[0024] 2. Different from the preparation of nanomaterials under liquid phase conditions by pulse laser focusing and ablation of target materials, the pulse laser induction generated in this device mainly involves the crushing, melting and modification of nanomaterials under parallel laser liquid phase conditions. Parallel laser can make full use of the uniformity of beam energy to optimize the nanomaterial synthesis process.

[0025] 3. After the inert gas is filled into the first container, it can prevent the raw material (solution containing nano material powder) from being oxidized.

[0026] 4. The computer can issue instructions to the control unit, and the control unit sends a pulse signal to the laser (the laser itself has a driver). At the same time, the control unit also sends a signal to the drive unit, and the drive unit controls the operation of the solenoid valve, the first pump, the second pump, and the third pump, thereby making the entire pulse laser induced preparation of nanomaterials more automated and controlling the entire process more accurately, thereby achieving high-precision automatic batch preparation or modified batch preparation of nanomaterials.

[0027] 5. Pulsed laser preparation of nanomaterials under liquid phase conditions is a green, low-cost and easy-to-operate method. This method mainly utilizes the interaction between laser and solution and medium to produce local non-equilibrium process. Through the process of energy concentration and differentiation, it can efficiently and quickly prepare or modify new nanomaterials. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a schematic diagram of the structure of the device for preparing nanomaterials by pulse laser induction according to the present invention.

[0029] Figure 2 It is a schematic structural diagram of the continuous dripping unit of the present invention.

[0030] In the figure, 100, the first container; 110, the dropper; 120, the solenoid valve; 200, the second container; 300, the laser; 410, the convex lens; 420, the concave lens; 500, the gas cylinder; 510, the gas pipe; 610, the reagent bottle; 620, the first pipeline; 630, the first pump; 640, the mixing bottle; 650, the second pipeline; 660, the second pump; 670, the agitator; 700, the liquid collecting bottle; 710, the third pipeline; 720, the third pump; 810, the drive unit; 820, the control unit; 830, the computer. DETAILED DESCRIPTION

[0031] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0032] like Figure 1-2 As shown, a device for preparing nanomaterials by pulsed laser induction under liquid phase conditions includes: a continuous dripping unit and a laser 300, wherein the continuous dripping unit includes a first container 100 and a second container 200, wherein the outlet of the first container 100 has a dropper 110, the second container 200 is located below the dropper 110, and an electromagnetic valve 120 for controlling the flow rate of liquid in the dropper 110 is provided between the outlet of the first container 100 and the dropper 110; the laser 300 generates laser in a working state and the laser is emitted toward the dropper 110.

[0033] The first container 100 is preferably a pear-shaped bottle, the upper end of the pear-shaped bottle has a porous stopper, the lower end of the pear-shaped bottle has a dropper 110 at the outlet, and the solenoid valve 120 is located between the dropper 110 and the outlet. The solenoid valve 120 can control the opening and closing of the outlet of the pear-shaped bottle, and can also accurately control the flow rate of the solution in the pear-shaped bottle entering the dropper 110.

[0034] The first container 100 and the second container 200 are both mounted on a bracket and arranged correspondingly up and down. The solution in the first container 100 contains nano material powder, and the solution continuously drips from the dropper 110 to the second container 200. During the dripping process, the laser generated by the laser 300 can be directed to the dropper 110 and induce the solution in the dropper 110. The interaction between the laser and the solution and the medium produces a local non-equilibrium process. Through the process of energy concentration and differentiation, new nano materials can be efficiently and quickly prepared in batches or modified in batches.

[0035] A safe, controllable and effective continuous batch preparation technology for nanomaterials is proposed, which can be used for batch preparation or modified batch preparation of nanomaterials, which not only improves the preparation efficiency but also simplifies the preparation steps.

[0036] The device also includes a convex lens 410 and a concave lens 420, which are located on the path of the laser generated by the laser 300 and are arranged in sequence along the emission direction of the laser. In a working state, the pulsed laser emitted by the laser 300 induces the liquid dripping in the dropper 110 after being contracted by the convex lens 410 and the concave lens 420.

[0037] The convex lens 410 can converge light to make the laser more concentrated, and the concave lens 420 has a divergent effect on light, so that the converged laser tends to be parallel. The laser emitted by the laser 300 is narrowed by the convex lens 410 and the concave lens 420 to obtain parallel pulsed laser.

[0038] It should be noted that the convex lens 410 and the concave lens 420 are arranged in sequence along the emission direction of the laser to form a structure that can focus the light. The focused parallel pulse laser induces the solution dripping from the dropper 110 at a vertical angle, wherein the optical focus reduction follows the classical Galilean and Keplerian inverted beam expansion structures.

[0039] Different from the preparation of nanomaterials under liquid phase conditions by pulsed laser focusing and ablation of targets, the pulsed laser induction generated in this device mainly involves the crushing, melting and modification of nanomaterials under parallel laser liquid phase conditions. Parallel laser can make full use of the uniformity of beam energy to optimize the nanomaterial synthesis process.

[0040] Preferably, the device further comprises a gas cylinder 500 for filling the first container 100 with an inert gas, and the gas cylinder 500 is connected to the first container 100 via a gas pipe 510 .

[0041] After the inert gas is filled into the first container 100, it can prevent the raw material (solution containing nanomaterial powder) from being oxidized. The inert gas specifically refers to one or more inert gases such as helium (He), neon (Ne), argon (Ar), krypton (Kr), and xenon (Xe).

[0042] The device further comprises a raw material supply unit for injecting a solution containing nano material powder into the first container 100 , and the raw material supply unit is connected to the first container 100 .

[0043] The raw material supply unit includes a mixing bottle 640 and at least two reagent bottles 610. The reagent bottle 610 is connected to the mixing bottle 640 via a first pipeline 620. The mixing bottle 640 is connected to the first container 100 via a second pipeline 650. The first pipeline 620 is provided with a first pump 630, and the second pipeline 650 is provided with a second pump 660.

[0044] It should be pointed out that the first pump 630 and the second pump 660 can preferably be peristaltic pumps or micro pumps, wherein the hoses at both ends of the first pump 630 are respectively connected to the reagent bottle 610 and the mixing bottle 640 to form a first pipeline 620, and the hoses at both ends of the second pump 660 are respectively connected to the mixing bottle 640 and the first container 100 to form a second pipeline 650. The first pump 630 and the second pump 660 can transport liquid and control the flow rate of the liquid.

[0045] The raw material supply unit further includes a stirrer 670 , and the mixing bottle 640 is disposed on the stirrer 670 ; in a working state, the stirrer 670 stirs the solution in the mixing bottle 640 .

[0046] One of the two reagent bottles 610 can be placed in a solution containing nanomaterial powder, and the other can be placed in a reaction reagent (reaction reagent may not be added). Under the action of the first pump 630, the solution and reaction reagent in the reagent bottle 610 are pumped into the mixing bottle 640 and stirred evenly, and then continuously replenished into the first container 100 according to the set flow rate, so as to continuously provide raw materials for batch preparation of nanomaterials.

[0047] The device further includes a liquid collecting bottle 700, which is connected to the second container 200 via a third pipeline 710, and the third pipeline 710 is provided with a third pump 720. The liquid collecting bottle 700 is used to collect the solution with the reaction product in the second container 200, and the third pump 720 extracts the solution in the second container 200 into the liquid collecting bottle 700 via the third pipeline 710.

[0048] It should be pointed out that in the actual structure, the ends of the second pipeline 650 and the air pipe 510 are inserted into the porous bottle stopper at the upper end of the first container 100 .

[0049] The device also includes a driving unit 810, a control unit 820 and a computer 830, wherein the control unit 820 is electrically connected to the computer 830, the laser 300 is electrically connected to the control unit 820, the driving unit 810 is electrically connected to the control unit 820, and the first pump 630, the second pump 660, the third pump 720 and the solenoid valve 120 are all electrically connected to the driving unit 810; in a working state, the computer 830 sends a pulse signal to the laser 300 through the control unit 820, and at the same time sends a control signal to the driving unit 810 through the control unit 820 to control the switch and flow rate of the first pump 630, the second pump 660, the third pump 720 and the solenoid valve 120.

[0050] The driving unit 810 is actually the driver of each pump and the solenoid valve 120, and the driving unit 810 also integrates a power supply. Simply put, the driving unit 810 can accurately control the flow of the solenoid valve 120, the first pump 630, the second pump 660 and the third pump 720; the control unit 820 specifically refers to a commonly used single-chip microcomputer chip, a digital signal processing chip, a system-level chip, a field programmable gate array chip, a complex programmable logic chip controller, etc.

[0051] When working, the computer 830 can issue instructions to the control unit 820, and the control unit 820 sends a pulse signal to the laser 300 (the laser 300 itself has a driver). At the same time, the control unit 820 also sends a signal to the drive unit 810, and the drive unit 810 controls the operation of the solenoid valve 120, the first pump 630, the second pump 660 and the third pump 720, thereby making the entire pulse laser induced preparation of nanomaterials process more automated and controlling the entire process more accurately, thereby achieving high-precision automatic batch preparation or modified batch preparation of nanomaterials.

[0052] like Figure 1-2 As shown, a method for preparing nanomaterials by pulsed laser induction under liquid phase conditions is also proposed, including the device for preparing nanomaterials by pulsed laser induction under liquid phase conditions, and also including the following steps:

[0053] S1: A solution containing nanomaterial powder and a reaction reagent are respectively placed in two reagent bottles 610, and the computer 830 drives the first pump 630 through the control unit 820 and the driving unit 810 to pump the solution in the reagent bottle 610 into the mixing bottle 640 at a set flow rate, and the stirrer 670 stirs the solution in the mixing bottle 640;

[0054] S2: The computer 830 drives the second pump 660 through the control unit 820 and the driving unit 810 to pump the mixed solution in the mixing bottle 640 into the first container 100 at a set flow rate;

[0055] S3: The computer 830 turns on the laser 300 through the control unit 820, and the laser 300 emits a pulse laser toward the dropper 110. The computer 830 turns on the solenoid valve 120 through the control unit 820 and the driving unit 810 and controls the flow rate of the solution flowing out of the first container 100. The solution in the first container 100 drips into the second container 200 through the dropper 110 at the set flow rate. The solution dripping from the dropper 110 is induced by the pulse laser, and the product induced by the pulse laser falls into the second container 200.

[0056] S4: The computer 830 drives the third pump 720 through the control unit 820 and the driving unit 810 to pump the product solution in the second container 200 into the liquid collecting bottle 700 at a set flow rate.

[0057] Pulsed laser preparation of nanomaterials under liquid phase conditions is a green, low-cost and easy-to-operate method. This method mainly utilizes the interaction between laser and solution and medium to produce local non-equilibrium process. Through the process of energy concentration and differentiation, it can efficiently and quickly prepare or modify new nanomaterials.

[0058] Preferably, in step S2 , if an inert gas environment is required in the first container 100 during the preparation process, the gas cylinder 500 is opened, and the inert gas in the gas cylinder 500 enters into the first container 100 .

[0059] Example 1: Laser-induced batch preparation of silicon nanoparticles

[0060] The capacity of the reagent bottle 610 is selected to be 500mL. One reagent bottle 610 is added with 10mg of amorphous nano powder with a particle size of 100nm and filled with 500mL of deionized water. No reagent is added to the other reagent bottle 610. The capacity of the mixing bottle 640 is selected to be 500mL. The capacity of the first container 100 is selected to be 500mL. The capacity of the second container 200 is selected to be 500mL. The capacity of the liquid collecting bottle 700 is selected to be 1000mL. The control flow rate of the first pump 630, the second pump 660 and the third pump 720 is 1mL / s. The other reagent bottle 610 is not added with reagent. 10 The first pump 630 corresponding to the position 10 is not turned on; the solenoid valve 120 controls the flow rate to be 1 mL / s; the pulse laser selects a wavelength of 355 nm (silicon absorbs best in the ultraviolet band), a pulse width of 10 ns, an energy of 50 mJ, and a spot size of 10 mm; the combined beam reduction ratio of the concave lens 420 and the convex lens 410 is 10:1, the designed focal length of the concave lens 420 is -15 mm, the focal length of the convex lens 410 is 150 mm, the distance between the two lenses is 135 mm, and the lens materials are all laser-resistant fused quartz materials; the inert gas in the gas cylinder 500 is argon (Ar) gas.

[0061] The specific preparation steps are as follows:

[0062] Step 1: Turn on the first pump 630 for 100 seconds, control its flow rate to 1 mL / s, extract 100 mL of solution from the reagent bottle 610 into the mixing bottle 640, and turn on the stirrer 670;

[0063] Step 2: Turn on the second pump 660 to extract 100 mL of solution in the mixing bottle 640 into the first container 100, and turn on the gas cylinder 500 to pass the inert gas argon into the first container 100;

[0064] Step 3: Turn on the laser 300, set the working time to 120s, open the solenoid valve 120 within 20s, control the flow rate of the solution out of the first container 100 to be 1mL / s, and drip 100mL of the product into the second container 200;

[0065] Step 4: Turn on the third pump 720 to extract 100 mL of product solution in the second container 200 into the liquid collection bottle 700;

[0066] Step 5: The computer 830 controls the entire system to cycle through steps 1-4 until the fifth cycle is completed;

[0067] Step 6: Turn off the first pump 630 and the second pump 660 ; then, when no mixed liquid flows out of the first container 100 , close the solenoid valve 120 , then turn off the laser 300 , and finally turn off the third pump 720 and the gas cylinder 500 .

[0068] Example 2: Laser-induced batch modification of silicon nanoparticles to achieve surface modification with gold shell

[0069] The capacity of the reagent bottle 610 is selected to be 500mL. 10mg of amorphous nanopowder with a particle size of 100nm is added to one reagent bottle 610, and 500mL of deionized water is added; 0.5mg of 500mL of tetrachloroauric acid solution is added to another reagent bottle 610, the capacity of the mixing bottle 640 is selected to be 500mL, the capacity of the first container 100 is selected to be 500mL, the capacity of the second container 200 is selected to be 500mL, and the capacity of the liquid collecting bottle 700 is selected to be 1000mL; the control flow rate of the first pump 630, the second pump 660 and the third pump 720 is 1mL / s, and the other The first pump 630 corresponding to the reagent bottle 610 is not turned on; the solenoid valve 120 controls the flow rate to be 1 mL / s; the pulse laser selects a wavelength of 532 nm (silicon and gold both have effective absorption at 532 nm), a pulse width of 10 ns, and an energy of 100 mJ; the spot size is 5 mm; the combined beam reduction ratio of the concave lens 420 and the convex lens 410 is 10:1, the designed focal length of the concave lens 420 is -30 mm, the focal length of the convex lens 410 is 150 mm, the distance between the two lenses is 120 mm, and the lens materials are all laser-resistant fused quartz materials; the inert gas in the gas cylinder 500 is helium (He) gas.

[0070] The specific preparation steps are as follows:

[0071] Step 1: Turn on the first pump 630 for 100 seconds, control its flow rate to 1 mL / s, extract 100 mL of solution from the two reagent bottles 610 into the mixing bottle 640, and turn on the stirrer 670;

[0072] Step 2: Turn on the second pump 660 to extract 200 mL of solution in the mixing bottle 640 into the first container 100, and turn on the gas cylinder 500 to let the inert gas helium flow into the first container 100;

[0073] Step 3: Turn on the laser 300, set the working time to 420s, open the solenoid valve 120 within 20s, control the flow rate of the solution out of the first container 100 to be 0.5mL / s, and drip 200mL of the product into the second container 200;

[0074] Step 4: Turn on the third pump 720 to extract 200 mL of product solution in the second container 200 into the liquid collection bottle 700;

[0075] Step 5: The computer 830 controls the entire system to cycle through steps 1-4 until the fifth cycle is completed;

[0076] Step 6: Turn off the first pump 630 and the second pump 660 ; then, when no mixed liquid flows out of the first container 100 , close the solenoid valve 120 , then turn off the laser 300 , and finally turn off the third pump 720 and the gas cylinder 500 .

[0077] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, etc.) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0078] In addition, in the present invention, the descriptions such as "first", "second", "one", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.

[0079] In the present invention, unless otherwise clearly stipulated and limited, the terms "connected", "fixed", etc. should be understood in a broad sense. For example, "fixed" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly limited.

[0080] In addition, the technical solutions between the various embodiments of the present invention can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

Claims

1. A device for preparing nanomaterials by pulsed laser induction under liquid phase conditions, characterized in that: include: A continuous dripping unit, comprising a first container (100) and a second container (200), wherein the outlet of the first container (100) is provided with a dripping tube (110), the second container (200) is located below the dripping tube (110), and an electromagnetic valve (120) is provided between the outlet of the first container (100) and the dripping tube (110) for controlling the flow rate of liquid in the dripping tube (110); A laser (300), wherein the laser (300) generates laser light in a working state and irradiates the laser light toward the dropper (110).

2. The device for preparing nanomaterials by pulsed laser induction under liquid phase conditions according to claim 1, characterized in that: It also includes a convex lens (410) and a concave lens (420), wherein the convex lens (410) and the concave lens (420) are located on the path of the laser generated by the laser (300) and are arranged in sequence along the emission direction of the laser; in a working state, the pulsed laser emitted by the laser (300) induces the liquid dripping in the dropper (110) after being contracted by the convex lens (410) and the concave lens (420).

3. The device for preparing nanomaterials by pulsed laser induction under liquid phase conditions as claimed in claim 1, characterized in that: It also includes a gas cylinder (500) for filling the first container (100) with an inert gas, and the gas cylinder (500) is connected to the first container (100) via a gas pipe (510).

4. The device for preparing nanomaterials by pulsed laser induction under liquid phase conditions as claimed in claim 1, characterized in that: It also comprises a raw material supply unit for injecting a solution containing nano material powder into the first container (100), and the raw material supply unit is connected to the first container (100).

5. The device for preparing nanomaterials by pulsed laser induction under liquid phase conditions as claimed in claim 4, characterized in that: The raw material supply unit includes a mixing bottle (640) and at least two reagent bottles (610), the reagent bottle (610) is connected to the mixing bottle (640) via a first pipeline (620), the mixing bottle (640) is connected to the first container (100) via a second pipeline (650), the first pipeline (620) is provided with a first pump (630), and the second pipeline (650) is provided with a second pump (660).

6. The device for preparing nanomaterials by pulsed laser induction under liquid phase conditions as claimed in claim 5, characterized in that: The raw material supply unit further comprises a stirrer (670), and the mixing bottle (640) is arranged on the stirrer (670); in a working state, the stirrer (670) stirs the solution in the mixing bottle (640).

7. The device for preparing nanomaterials by pulsed laser induction under liquid phase conditions as claimed in claim 5, characterized in that: It also includes a liquid collecting bottle (700), wherein the liquid collecting bottle (700) is connected to the second container (200) via a third pipeline (710), and the third pipeline (710) is provided with a third pump (720).

8. The device for preparing nanomaterials by pulsed laser induction under liquid phase conditions as claimed in claim 7, characterized in that: The invention also includes a driving unit (810), a control unit (820) and a computer (830), wherein the control unit (820) is electrically connected to the computer (830), the laser (300) is electrically connected to the control unit (820), the driving unit (810) is electrically connected to the control unit (820), and the first pump (630), the second pump (660), the third pump (720) and the solenoid valve (120) are all electrically connected to the driving unit (810); in a working state, the computer (830) sends a pulse signal to the laser (300) through the control unit (820), and at the same time sends a control signal to the driving unit (810) through the control unit (820) to control the switch and flow rate of the first pump (630), the second pump (660), the third pump (720) and the solenoid valve (120).

9. A method for preparing nanomaterials by pulsed laser induction under liquid phase conditions, characterized in that: The device for preparing nanomaterials by pulsed laser induction under liquid phase conditions as claimed in any one of claims 1 to 8 further comprises the following steps: S1: A solution containing nano material powder and a reaction reagent are respectively placed in two reagent bottles (610), a computer (830) drives a first pump (630) through a control unit (820) and a drive unit (810) to pump the solution in the reagent bottle (610) into a mixing bottle (640) at a set flow rate, and a stirrer (670) stirs the solution in the mixing bottle (640); S2: The computer (830) drives the second pump (660) through the control unit (820) and the driving unit (810) to pump the mixed solution in the mixing bottle (640) into the first container (100) at a set flow rate; S3: The computer (830) turns on the laser (300) through the control unit (820), and the laser (300) emits a pulse laser toward the dropper (110), and the computer (830) turns on the solenoid valve (120) through the control unit (820) and the drive unit (810) and controls the flow rate of the solution flowing out of the first container (100), and the solution in the first container (100) drips into the second container (200) through the dropper (110) at the set flow rate, and the solution dripping from the dropper (110) is induced by the pulse laser, and the product induced by the pulse laser falls into the second container (200); S4: The computer (830) drives the third pump (720) through the control unit (820) and the driving unit (810) to pump the product solution in the second container (200) into the liquid collection bottle (700) at a set flow rate.

10. The method for preparing nanomaterials by pulsed laser induction under liquid phase conditions according to claim 9, characterized in that: In step S2, if there is a need for an inert gas environment in the first container (100) during the preparation process, the gas cylinder (500) is opened, and the inert gas in the gas cylinder (500) enters the first container (100).