Lithium extraction resin, preparation method and application thereof, and method for recovering lithium in lithium-containing feed liquid
By using the alkyl salicylate ion exchanger in the porous spherical lithium extraction resin, efficient recovery of lithium is achieved, solving the problems of difficult separation of lithium and other alkali metal ions and high energy consumption, and improving the efficiency of lithium recovery. and economical, avoiding environmental pollution.
Patent Information
- Application Number
- CN202410797148.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-20
AI Technical Summary
In existing lithium recovery technology, it is difficult to separate lithium from other alkali metal ions, resulting in low lithium extraction efficiency and high energy consumption. In addition, the high content of impurity ions in traditional methods makes it impossible to produce high-value lithium carbonate products.
Porous spherical lithium extraction resin is used. The resin contains alkyl salicylate as an ion exchanger. It achieves efficient recovery of lithium through adsorption and desorption processes, overcoming the problems of difficult phase separation and high energy consumption.
The lithium extraction rate is improved, energy consumption is reduced, and the resin can be recycled multiple times, significantly reducing operating costs while avoiding environmental problems caused by the volatilization of organic solvents.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical separation, and specifically relates to a lithium extraction resin, a preparation method and application thereof, and a method for recovering lithium from a lithium-containing feed liquid. Background Art
[0002] Lithium is an important rare metal. It is widely used in batteries, metallurgy, aerospace, medicine, military and other fields due to its excellent physical and chemical properties such as low density and strong electrochemical activity. Driven by the new energy technology revolution represented by high-energy lithium batteries and emerging technologies such as lithium-aluminum alloys and controlled thermonuclear fusion, the global market demand for lithium is growing rapidly, and the status of lithium resources in the world is gradually improving.
[0003] At present, Li2CO3 is mainly obtained by reacting concentrated lithium-rich solution with sodium carbonate to obtain lithium carbonate and lithium precipitation mother liquor. Due to the large solubility product of Li2CO3, the lithium precipitation rate in the system is generally only 70-80%. The traditional method of recovering lithium from lithium precipitation mother liquor is to first neutralize the lithium precipitation mother liquor with sulfuric acid to remove CO3 2- Then, the neutralized lithium precipitation mother liquor is evaporated and concentrated, and anhydrous sodium sulfate is separated by crystallization for secondary lithium precipitation; but due to the impurity ions Na + , K + The high content can only produce industrial secondary lithium carbonate products with low value, which is a long-standing and unresolved problem in the lithium industry. Therefore, it is urgent to improve and upgrade the existing lithium carbonate production technology.
[0004] Regarding the separation of lithium from other alkali metal ions in lithium precipitation mother liquor, patent documents CN115786735A and CN112342405A currently report methods for extracting lithium from alkaline solutions using a β-diketone-organophosphine extraction system, and patent document CN115433830A reports methods for extracting lithium from alkaline lithium-containing solutions using a salicylic acid alkyl ester-organophosphine extraction system, both of which achieve good separation effects. However, the above-mentioned extraction systems are prone to phase separation difficulties when the extracted metal ion load is high, thereby limiting the large-scale industrial application of the β-diketone / salicylic acid alkyl ester-organophosphine extraction system. Summary of the invention
[0005] The purpose of the present invention is to provide a lithium extraction resin and a preparation method and application thereof, and a method for recovering lithium from a lithium-containing liquid. The lithium extraction resin provided by the present invention can overcome the problem of difficult phase separation and has a good extraction effect.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a lithium extraction resin, comprising a resin and an ion exchanger distributed in the resin; the ion exchanger is an alkyl salicylate;
[0008] The lithium extraction resin is in a porous spherical or quasi-spherical shape, and has a particle size of 100 to 200 meshes.
[0009] Preferably, the resin is a polystyrene resin;
[0010] The salicylic acid alkyl ester includes one or more of octyl salicylate, propyl salicylate, butyl salicylate, pentyl salicylate and hexyl salicylate; the mass percentage of the ion exchanger in the lithium extraction resin is 10-60%.
[0011] Preferably, the pore volume of the lithium extraction resin is greater than 2 mL / g and the specific surface area is 500 m 2 / g or more, and the average pore diameter is or more than 10nm.
[0012] The present invention also provides a method for preparing the lithium extraction resin described in the above technical solution, comprising the following steps:
[0013] The monomer, ion exchanger, cross-linking agent, initiator and porogen are first mixed to obtain an organic phase; the ion exchanger is alkyl salicylate;
[0014] secondly mixing the dispersant, the surfactant and water to obtain an aqueous phase;
[0015] The organic phase and the aqueous phase are thirdly mixed to obtain a reaction solution;
[0016] The reaction solution is subjected to a polymerization reaction to obtain the lithium-extracting resin.
[0017] Preferably, the monomer is styrene;
[0018] The cross-linking agent is divinylbenzene;
[0019] The initiator is benzoyl peroxide, azobisisobutyl cyanide, cumene hydroperoxide or lauroyl peroxide;
[0020] The porogen is sodium thiocyanate, sodium bicarbonate, sodium carbonate, n-butyl ether or toluene;
[0021] The dispersant is gelatin or polyvinyl alcohol;
[0022] The surfactant is sodium dodecyl sulfate or Triton.
[0023] Preferably, the volume ratio of the monomer to the cross-linking agent is 1:0.5-1.5;
[0024] The volume ratio of the monomer to the reaction liquid is 1:10-20;
[0025] The mass percentage of the ion exchanger in the organic phase is 10-60%.
[0026] The present invention also provides the use of the lithium extraction resin described in the above technical solution or the lithium extraction resin obtained by the preparation method described in the above technical solution in recovering lithium.
[0027] The present invention also provides a method for recovering lithium from a lithium-containing liquid, comprising the following steps:
[0028] Passing the lithium-containing feed liquid into a lithium-extracting resin for adsorption to obtain an adsorption tail liquid and a lithium-rich resin; the lithium-extracting resin is the lithium-extracting resin described in the above technical solution or the lithium-extracting resin obtained by the preparation method described in the above technical solution;
[0029] The acid solution is passed into the lithium-rich resin for desorption to obtain a lithium desorption solution.
[0030] Preferably, the lithium concentration in the lithium-containing liquid is 0.05 to 10 g / L; the flow rate of the lithium-containing liquid is 2 to 5 BV / h;
[0031] The ratio of the lithium concentration in the adsorption tail liquid to the lithium concentration in the lithium-containing feed liquid is 1:10-100; the adsorption is stopped when the lithium concentration in the adsorption tail liquid reaches 0.005-1 g / L.
[0032] Preferably, the acid solution includes one or more of hydrochloric acid solution, nitric acid solution and sulfuric acid solution; the hydrogen ion concentration of the acid solution is 0.05 to 6 mol / L;
[0033] The acid solution is introduced at a flow rate of 0.5 to 2 BV / h.
[0034] The present invention provides a lithium extraction resin, comprising a resin and an ion exchanger distributed in the resin; the ion exchanger is an alkyl salicylate; the lithium extraction resin is porous spherical or quasi-spherical, with a particle size of 100 to 200 meshes. The lithium extraction resin provided by the present invention can be used as a leaching resin in the lithium recovery process, which can not only prevent the loss of the ion exchanger, but also effectively overcome the problem of phase separation difficulties in the liquid extraction system, improve the extraction rate, and reduce energy consumption. In addition, the resin can be recycled for multiple times, greatly reducing the operating cost.
[0035] The recovery method provided by the present invention has a simple process and is easy to operate. It achieves the high selectivity of the solvent extraction method and has the advantages of simple equipment and high efficiency of the ion exchange method. It can improve the recovery rate and reduce energy consumption. In addition, the process does not require the use of co-extractants and diluents, thus avoiding environmental problems caused by the volatilization of organic solvents. DETAILED DESCRIPTION
[0036] The present invention provides a lithium extraction resin, comprising a resin and an ion exchanger distributed in the resin; the ion exchanger is an alkyl salicylate;
[0037] The lithium extraction resin is in a porous spherical or quasi-spherical shape, and has a particle size of 100 to 200 meshes.
[0038] In the present invention, unless otherwise specified, all raw material components are commercially available products known to those skilled in the art.
[0039] In the present invention, the resin is preferably a polystyrene resin.
[0040] In the present invention, the alkyl chain in the alkyl salicylate is preferably C3-C8; the alkyl salicylate preferably includes one or more of octyl salicylate, propyl salicylate, butyl salicylate, pentyl salicylate and hexyl salicylate, and more preferably one or more of octyl salicylate, butyl salicylate and pentyl salicylate; the octyl salicylate preferably includes isooctyl salicylate and / or n-octyl salicylate; the butyl salicylate is preferably n-butyl salicylate; the pentyl salicylate is preferably isopentyl salicylate; when the alkyl salicylate is two or more of the above types, the present invention has no special limitation on the ratio of the alkyl salicylate; the alkyl salicylate is soluble in styrene-divinylbenzene system; the mass percentage of the ion exchanger in the lithium extraction resin is preferably 10-60%, and more preferably 15-50%.
[0041] In the present invention, the color of the lithium extraction resin is preferably opaque white; the particle size is 100-200 mesh, preferably 100-200 mesh; the pore volume of the lithium extraction resin is preferably 2 mL / g or more, more preferably 3-5 mL / g; the specific surface area is preferably 500 m 2 / g or more, more preferably 600 to 800 m 2 / g; the average pore diameter is preferably 10 nm or more, more preferably 10 to 12 nm.
[0042] The present invention also provides a method for preparing the lithium extraction resin described in the above technical solution, comprising the following steps:
[0043] The monomer, ion exchanger, cross-linking agent, initiator and porogen are first mixed to obtain an organic phase; the ion exchanger is alkyl salicylate;
[0044] secondly mixing the dispersant, the surfactant and water to obtain an aqueous phase;
[0045] The organic phase and the aqueous phase are thirdly mixed to obtain a reaction solution;
[0046] The reaction solution is subjected to a polymerization reaction to obtain the lithium-extracting resin.
[0047] The invention first mixes monomers, ion exchangers, crosslinking agents, initiators and porogens to obtain an organic phase.
[0048] In the present invention, the monomer is preferably styrene; the use of styrene as a monomer has the advantage of excellent alkali resistance, and is suitable for the extraction of lithium-containing liquid.
[0049] In the present invention, the alkyl chain in the alkyl salicylate is preferably C3-C8; the alkyl salicylate preferably includes one or more of octyl salicylate, propyl salicylate, butyl salicylate, pentyl salicylate and hexyl salicylate, and more preferably one or more of octyl salicylate, butyl salicylate and pentyl salicylate; the octyl salicylate preferably includes isooctyl salicylate and / or n-octyl salicylate; the butyl salicylate is preferably n-butyl salicylate; the pentyl salicylate is preferably isopentyl salicylate; when the alkyl salicylate is two or more of the above types, the present invention has no special limitation on the ratio of the alkyl salicylate; the alkyl salicylate is soluble in a styrene-divinylbenzene system.
[0050] In the present invention, the cross-linking agent is preferably divinylbenzene; the volume ratio of the monomer to the cross-linking agent is preferably 1:0.5-1.5, more preferably 1:1-1.5.
[0051] In the present invention, the initiator is preferably benzoyl peroxide, azobisisobutyl cyanide, cumene hydroperoxide or lauroyl peroxide, more preferably benzoyl peroxide, azobisisobutyl cyanide or cumene hydroperoxide;
[0052] The mass ratio of the monomer volume to the initiator is preferably 25 mL: 0.25-1 g, more preferably 25 mL: 0.4-0.8 g.
[0053] In the present invention, the porogen is preferably sodium thiocyanate, sodium bicarbonate, sodium carbonate, n-butyl ether or toluene, more preferably sodium thiocyanate, sodium bicarbonate or sodium carbonate; the mass ratio of the volume of the monomer to the porogen is preferably 25 mL: 0.1-0.5 g, more preferably 25 mL: 0.2-0.4 g.
[0054] In the present invention, the mass percentage of the ion exchanger in the organic phase is preferably 10 to 60%, more preferably 15 to 50%.
[0055] In the present invention, the first mixing process is preferably: first adding the ion exchanger to the monomer, then mixing with the cross-linking agent and the initiator for a first stirring, and finally mixing with the porogen for a second stirring; the present invention has no special limitation on the first stirring process, and the initiator can be completely dissolved in a manner well known to those skilled in the art; the present invention has no special limitation on the second stirring process, and the organic phase can be made uniform and stable in a manner well known to those skilled in the art.
[0056] In the present invention, the dispersant, the surfactant and water are mixed for the second time to obtain an aqueous phase.
[0057] In the present invention, the dispersant is preferably gelatin or polyvinyl alcohol; the mass ratio of the dispersant to water is preferably 0.5 to 1:300, more preferably 0.5 to 1:300.
[0058] In the present invention, the surfactant is preferably sodium dodecyl sulfate or Triton; the model of the Triton is preferably TX-100; the mass ratio of the surfactant to water is preferably 0.1 to 0.25:300, more preferably 0.15 to 0.2:300.
[0059] The present invention does not have any special limitation on the second mixing process, and a method well known to those skilled in the art may be used.
[0060] After obtaining the organic phase and the aqueous phase, the present invention thirdly mixes the organic phase and the aqueous phase to obtain a reaction solution.
[0061] The present invention does not have any special limitation on the third mixing process, and a method well known to those skilled in the art may be adopted.
[0062] In the present invention, the volume ratio of the monomer to the reaction solution is preferably 1:10-20, more preferably 1:12-18.
[0063] After obtaining the reaction solution, the present invention performs a polymerization reaction on the reaction solution to obtain the lithium-extracting resin.
[0064] In the present invention, the polymerization reaction is preferably suspension polymerization; the polymerization reaction preferably includes a first stage and a second stage carried out in sequence; the temperature of the first stage is preferably 80-85°C, the time is preferably 0.25-1h, and more preferably 0.5h; the temperature of the second stage is preferably 90-95°C, more preferably 90°C, and the time is preferably 2-4h; the role of the second stage is to make the residual initiator and monomer react completely; the polymerization reaction is carried out under stirring conditions; the present invention does not have any special limitation on the stirring process, and the method familiar to those skilled in the art can be used.
[0065] In the present invention, after the polymerization reaction, it is preferred to include cooling, washing, filtration and drying in sequence; the present invention does not have any special limitation on the cooling process, and cooling to below 50° C. can be carried out in a manner well known to those skilled in the art; the present invention does not have any special limitation on the washing process, and washing can be carried out in a manner well known to those skilled in the art until the washing liquid is clarified; the present invention does not have any special limitation on the filtration and drying processes, and methods well known to those skilled in the art can be used.
[0066] The lithium extraction resin provided by the present invention can be used as a leaching resin in the lithium recovery process, which can not only prevent the loss of ion exchangers, but also effectively overcome the problem of phase separation difficulties, improve the extraction rate, and reduce energy consumption. In addition, the resin can be recycled for multiple times, greatly reducing the operating cost.
[0067] The present invention also provides the use of the lithium extraction resin described in the above technical solution or the lithium extraction resin obtained by the preparation method described in the above technical solution in recovering lithium.
[0068] The present invention also provides a method for recovering lithium from a lithium-containing liquid, comprising the following steps:
[0069] Passing the lithium-containing feed liquid into a lithium-extracting resin for adsorption to obtain an adsorption tail liquid and a lithium-rich resin; the lithium-extracting resin is the lithium-extracting resin described in the above technical solution or the lithium-extracting resin obtained by the preparation method described in the above technical solution;
[0070] The acid solution is passed into the lithium-rich resin for desorption to obtain a lithium desorption solution.
[0071] The present invention passes lithium-containing feed liquid into lithium-extracting resin for adsorption to obtain adsorption tail liquid and lithium-rich resin.
[0072] In the present invention, washing is preferably included before adsorption; the washing includes acid washing and alkali washing; the present invention does not have any special limitation on the process of acid washing and alkali washing, and methods familiar to those skilled in the art can be used; the purpose of the acid washing and alkali washing is to wash away the residual porogens, surfactants and ion exchangers remaining on the surface of the resin, so that the resin has a stable macroporous structure.
[0073] In the present invention, the lithium-extracting resin is preferably loaded into an ion exchange column before adsorption; the specification of the ion exchange column is Φ35mm×400mm; the filling amount is preferably 100-150g, more preferably 100-120g; the column diameter ratio is preferably 5-10, more preferably 6-9.
[0074] In the present invention, the lithium concentration in the lithium-containing solution is preferably 0.05-10 g / L, more preferably 0.1-5 g / L; the hydroxide ion concentration is preferably 0.01-6 mol / L, more preferably 0.1-5 g / L; the lithium-containing solution is preferably a lithium precipitation mother liquor; the inlet flow rate of the lithium-containing solution is preferably 2-5 BV / h, more preferably 3-4 BV / h.
[0075] In the present invention, the ratio of the lithium concentration in the adsorption tail liquid to the lithium concentration in the lithium-containing feed liquid is preferably 1:10-100, more preferably 1:20-80; the adsorption is stopped when the lithium concentration in the adsorption tail liquid preferably reaches 0.005-1 g / L, more preferably 0.005-0.05 g / L.
[0076] After obtaining the lithium-rich resin, the present invention passes an acid solution into the lithium-rich resin to perform desorption to obtain a lithium desorption solution.
[0077] In the present invention, washing is also included before desorption; the washing reagent is preferably water; the flow rate of the washing is preferably 0.5-5BV / h, more preferably 1-4BV / h; the time is preferably 10-60min, more preferably 30-60min; the reason for the washing is that after the adsorption mother liquor flows through the resin column for adsorption, there is residual mother liquor in the resin column, and the mother liquor contains impurities such as sodium and potassium. If water washing is not used, sodium and potassium will enter the desorption liquid during the desorption stage, and the sodium and potassium content in the desorption liquid is likely to exceed the standard, resulting in failure to achieve the purpose of preparing a relatively pure lithium solution.
[0078] In the present invention, the acid solution preferably includes one or more of hydrochloric acid solution, nitric acid solution and sulfuric acid solution, more preferably hydrochloric acid solution and / or sulfuric acid solution; the hydrogen ion concentration of the acid solution is preferably 0.05-6 mol / L, more preferably 0.1-5 mol / L; the inlet flow rate of the acid solution is preferably 0.5-2 BV / h, more preferably 1-2 BV / h.
[0079] In the present invention, desorption is stopped when the lithium concentration in the lithium desorption solution is preferably as low as 0.01 to 1 g / L, and more preferably 0.05 to 0.5 g / L.
[0080] In the present invention, the desorption is preferably followed by washing; the washing reagent is preferably water; the flow rate of the washing is preferably 0.5 to 5 BV / h, more preferably 1 to 4 BV / h; the time is preferably 10 to 60 min, more preferably 30 to 60 min; the purpose of the washing is to achieve the regeneration of the lithium extraction resin.
[0081] The recovery method provided by the present invention has a simple process and is easy to operate. It achieves the high selectivity of the solvent extraction method and has the advantages of simple equipment and high efficiency of the ion exchange method. It can improve the recovery rate and reduce energy consumption. In addition, the process does not require the use of co-extractants and diluents, thus avoiding environmental problems caused by the volatilization of organic solvents.
[0082] In order to further illustrate the present invention, the lithium extraction resin provided by the present invention, its preparation method and application, and the method for recovering lithium from lithium-containing liquid are described in detail below in conjunction with the embodiments, but they should not be understood as limiting the scope of protection of the present invention.
[0083] Example 1
[0084] Preparation of resin: In a dry beaker, add 50mL isooctyl salicylate, 25mL styrene, 25mL divinylbenzene and 0.25g initiator benzoyl peroxide, stir to dissolve the initiator completely. Add 0.5g porogen sodium thiocyanate, stir the above oil phase evenly and add it to a 500mL three-necked flask containing 300mL deionized water, 0.5g gelatin and 0.25g sodium dodecyl sulfonate, install a thermometer, condenser and electric stirrer, react at 80℃ for 0.5h, then heat to 90℃ for 3h to react the residual initiator and monomer completely. Cool to about 50℃, wash with deionized water until the water phase is clear, filter and dry for later use. The color of the obtained resin is opaque white, the content of isooctyl salicylate in the resin is 48.9%, the screening particle size is 100-200 mesh, the pore volume is 4.25 mL / g, and the specific surface area is preferably 824.3 m 2 / g, and the average pore size is 12.6nm.
[0085] Adsorption: Weigh 100g of leaching resin and wash it with dilute acid and dilute alkali several times in turn, then fill it into an ion exchange column with a column diameter ratio of 7. Pass the lithium precipitation mother liquor into the ion exchange column at a flow rate of 5BV / h for adsorption, wherein the lithium concentration in the lithium-containing liquid is 2g / L, the sodium concentration is 50g / L, and the hydroxide concentration is 0.1mol / L. When the lithium concentration of the outlet liquid reaches 0.05g / L, stop the adsorption. Wash the resin with water at a flow rate of 2BV / h for 30min, and proceed to the next step after washing.
[0086] Desorption: Use sulfuric acid to desorb the adsorbed resin, and the hydrogen ion concentration in the desorbent is 3 mol / L; pass the desorbent through the resin after lithium adsorption at a flow rate of 0.5 BV / h, and stop desorption when the lithium concentration of the outlet desorption liquid is less than 0.1 g / L.
[0087] Regeneration: After the adsorption and desorption process is completed, the resin is washed with water at a flow rate of 1.5BV / h for 30 minutes. After washing, the regenerated resin can enter the next cycle of adsorption process.
[0088] In this embodiment, the TOC value in the adsorption tail liquid is 12.0 mg / L, and the TOC value in the desorption liquid is 19.5 mg / L; the desorption rate of lithium in the desorption step is 99%, and the lithium concentration in the desorption liquid is 13 g / L.
[0089] Example 2
[0090] Preparation of resin: In a dry beaker, add 20mL isoamyl salicylate, 25mL styrene, 25mL divinylbenzene and 0.25g initiator azobisisobutyl cyanide, stir to dissolve the initiator completely. Add 0.5g porogen sodium thiocyanate, stir the above oil phase evenly and add it to a 500mL three-necked flask containing 300mL deionized water, 0.5g gelatin and 0.5g sodium dodecyl sulfonate, install a thermometer, condenser and electric stirrer, react at 80℃ for 0.5h, then heat to 90℃ for 2h to react the residual initiator and monomer completely. Cool to about 50℃, wash with deionized water until the water phase is clear, filter and dry for later use. The color of the obtained resin is opaque white, the content of isoamyl salicylate in the resin is 25.7%, the screening particle size is 100-200 mesh, the pore volume is 3.78 mL / g, and the specific surface area is preferably 810.4 m 2 / g, and the average pore size is 10.1nm.
[0091] Adsorption: Weigh 100g of leaching resin and wash it with dilute acid and dilute alkali several times in sequence, then fill it into an ion exchange column with a column diameter ratio of 7. Pass the lithium precipitation mother liquor into the ion exchange column at a flow rate of 2BV / h for adsorption, wherein the lithium concentration in the lithium-containing liquid is 0.1g / L, the sodium concentration is 10g / L, and the hydroxide concentration is 0.5mol / L. When the lithium concentration of the outlet liquid reaches 0.01g / L, stop the adsorption. Wash the resin with water at a flow rate of 2BV / h for 30min, and proceed to the next step after washing.
[0092] Desorption: Use sulfuric acid to desorb the adsorbed resin, and the hydrogen ion concentration in the desorbent is 3 mol / L; pass the desorbent through the resin after lithium adsorption at a flow rate of 0.5 BV / h, and stop desorption when the lithium concentration of the outlet desorption liquid is less than 0.1 g / L.
[0093] Regeneration: After the adsorption and desorption process is completed, the resin is washed with water at a flow rate of 1.0 BV / h for 30 minutes. After washing, the regenerated resin can enter the next cycle of adsorption process.
[0094] In this embodiment, the TOC value in the adsorption tail liquid is 15.5 mg / L, and the TOC value in the desorption liquid is 23.0 mg / L; the desorption rate of lithium in the desorption step is 99.3%, and the lithium concentration in the desorption liquid is 1.5 g / L.
[0095] Example 3
[0096] Preparation of resin: In a dry beaker, add 15mL of n-butyl salicylate, 25mL of styrene, 25mL of divinylbenzene and 0.5g of initiator lauroyl peroxide, and stir to completely dissolve the initiator. Add 0.5g of porogen sodium thiocyanate, stir the above oil phase evenly and add it to a 500mL three-necked flask containing 300mL of deionized water, 0.5g of gelatin and 0.5g of sodium dodecyl sulfonate, install a thermometer, condenser and electric stirrer, react at 85℃ for 1h, then heat to 90℃ for 2h to react the residual initiator and monomer completely. Cool to about 50℃, wash with deionized water until the water phase is clear, filter, dry and set aside. The color of the obtained resin is opaque white, the content of isooctyl salicylate in the resin is 20.1%, the screening particle size is 100-200 mesh, the pore volume is 5.10mL / g, and the specific surface area is preferably 794.3m 2 / g, and the average pore size is 10.9nm.
[0097] Adsorption: Weigh 100g of leaching resin and wash it with dilute acid and dilute alkali several times in turn, then fill it into an ion exchange column with a column diameter ratio of 7. Pass the lithium precipitation mother liquor into the ion exchange column at a flow rate of 2BV / h for adsorption, wherein the lithium concentration in the lithium-containing liquid is 5g / L, the sodium concentration is 70g / L, and the hydroxide concentration is 0.1mol / L. When the lithium concentration of the outlet liquid reaches 0.1g / L, stop the adsorption. Wash the resin with water at a flow rate of 0.5BV / h for 30min, and proceed to the next step after washing.
[0098] Desorption: Use sulfuric acid to desorb the resin after adsorption, and the hydrogen ion concentration in the desorbent is 6 mol / L; pass the desorbent through the resin after lithium adsorption at a flow rate of 0.5 BV / h, and stop desorption when the lithium concentration of the outlet desorption liquid is less than 0.1 g / L.
[0099] Regeneration: After the adsorption and desorption process is completed, the resin is washed with water at a flow rate of 0.5BV / h for 60 minutes. After washing, the regenerated resin can enter the next cycle of adsorption process.
[0100] In this embodiment, the TOC value in the adsorption tail liquid is 21.0 mg / L, and the TOC value in the desorption liquid is 30.5 mg / L; the desorption rate of lithium in the desorption step is 98.7%, and the lithium concentration in the desorption liquid is 10 g / L.
[0101] Example 4
[0102] Preparation of resin: In a dry beaker, add 15mL isooctyl salicylate and 15mL isoamyl salicylate, 25mL styrene, 25mL divinylbenzene and 0.5g initiator benzoyl peroxide, stir to dissolve the initiator completely. Add 0.5g porogen sodium thiocyanate, stir the above oil phase evenly and add it to a 500mL three-necked flask containing 300mL deionized water, 1.0g gelatin and 0.5g sodium dodecyl sulfonate, install a thermometer, condenser and electric stirrer, react at 85℃ for 1h, then heat to 95℃ for 2h to react the residual initiator and monomer completely. Cool to about 50℃, wash with deionized water until the water phase is clear, filter and dry for later use. The color of the obtained resin is opaque white, the content of isooctyl salicylate in the resin is 37.5%, the screening particle size is 100-200 mesh, the pore volume is 5.60 mL / g, and the specific surface area is preferably 763.2 m 2 / g, and the average pore size is 11.1nm.
[0103] Adsorption: Weigh 100g of leaching resin and wash it with dilute acid and dilute alkali several times in turn, then fill it into an ion exchange column with a column diameter ratio of 7. Pass the lithium precipitation mother liquor into the ion exchange column at a flow rate of 5BV / h for adsorption, wherein the lithium concentration in the lithium-containing liquid is 2.5g / L, the sodium concentration is 50g / L, and the hydroxide concentration is 0.8mol / L. When the lithium concentration of the outlet liquid reaches 0.5g / L, stop the adsorption. Wash the resin with water at a flow rate of 2BV / h for 30min, and proceed to the next step after washing.
[0104] Desorption: Use sulfuric acid to desorb the resin after adsorption, and the hydrogen ion concentration in the desorbent is 3 mol / L; pass the desorbent through the resin after lithium adsorption at a flow rate of 2BV / h, and stop desorption after measuring the lithium concentration of the outlet desorption liquid is less than 1g / L.
[0105] Regeneration: After the adsorption and desorption process is completed, the resin is washed with water at a flow rate of 5BV / h for 10 minutes. After washing, the regenerated resin can enter the next cycle of adsorption process.
[0106] In this embodiment, the TOC value in the adsorption tail liquid is 11.5 mg / L, and the TOC value in the desorption liquid is 31.7 mg / L; the desorption rate of lithium in the desorption step is 95.5%, and the lithium concentration in the desorption liquid is 25 g / L.
[0107] Example 5
[0108] Preparation of resin: In a dry beaker, add 15mL isoamyl salicylate, 25mL styrene, 25mL divinylbenzene and 0.25g initiator benzoyl peroxide, stir to completely dissolve the initiator. Add 0.5g porogen sodium bicarbonate, stir the above oil phase evenly and add it to a 500mL three-necked flask containing 300mL deionized water, 0.5g gelatin and 0.25g sodium dodecyl sulfonate. Install a thermometer, condenser and electric stirrer, react at 80℃ for 0.5h, then heat to 95℃ for 2h to react the residual initiator and monomer completely. Cool to about 50℃, wash with deionized water until the water phase is clear, filter and dry for later use. The color of the obtained resin is opaque white, the content of isooctyl salicylate in the resin is 23.0%, the screening particle size is 100-200 mesh, the pore volume is 3.25 mL / g, and the specific surface area is preferably 768.0 m 2 / g, and the average pore size is 12.0nm.
[0109] Adsorption: Weigh 100g of leaching resin and wash it with dilute acid and dilute alkali several times in turn, then fill it into an ion exchange column with a column diameter ratio of 7. Pass the lithium precipitation mother liquor into the ion exchange column at a flow rate of 2BV / h for adsorption, wherein the lithium concentration in the lithium-containing liquid is 0.05g / L, the sodium concentration is 10g / L, and the hydroxide concentration is 0.03mol / L. When the lithium concentration of the outlet liquid reaches 0.005g / L, stop the adsorption. Wash the resin with water at a flow rate of 1BV / h for 30min, and proceed to the next step after washing.
[0110] Desorption: Use sulfuric acid to desorb the resin after adsorption, and the hydrogen ion concentration in the desorbent is 0.05 mol / L; pass the desorbent through the resin after lithium adsorption at a flow rate of 0.5 BV / h, and stop desorption when the lithium concentration of the outlet desorption liquid is less than 0.01 g / L.
[0111] Regeneration: After the adsorption and desorption process is completed, the resin is washed with water at a flow rate of 0.5BV / h for 60 minutes. After washing, the regenerated resin can enter the next cycle of adsorption process.
[0112] In this embodiment, the TOC value in the adsorption tail liquid is 20.1 mg / L, and the TOC value in the desorption liquid is 33.9 mg / L; the desorption rate of lithium in the desorption step is 99.4%, and the lithium concentration in the desorption liquid is 0.8 g / L.
[0113] Comparative Example
[0114] Using isooctyl salicylate as an extractant, trialkylphosphine oxide as a co-extractant, and sulfonated kerosene as a diluent to obtain an extracted organic phase #1, wherein the concentration of isooctyl salicylate in the organic phase is 1.0 mol / L, the concentration of trialkylphosphine oxide is 1.0 mol / L, and the rest is sulfonated kerosene. Using benzoyltrifluoroacetone as an extractant, trialkylphosphine oxide as a co-extractant, and sulfonated kerosene as a diluent to obtain an extracted organic phase #2, wherein the concentration of benzoyltrifluoroacetone in the organic phase is 1.0 mol / L, the concentration of trialkylphosphine oxide is 1.0 mol / L, and the rest is sulfonated kerosene.
[0115] A lithium-containing solution with a lithium concentration of 0.05 g / L, a sodium concentration of 10 g / L, and a hydroxide concentration of 0.03 mol / L was taken as the extraction aqueous phase.
[0116] The above #1 extracted organic phase and #2 extracted organic phase were subjected to single-stage extraction with the extracted aqueous phase at an extraction ratio (O / A) = 1:1, and the extraction time was 15 min. After the extraction reached equilibrium, the phases were separated by standing to obtain #1 raffinate and #2 raffinate, respectively. The loaded organic phase was then stripped with 3 mol / L hydrochloric acid solution at a ratio (O / A) = 10:1 to obtain #1 stripping solution and #2 stripping solution.
[0117] The TOC values in the raffinate and stripping liquid were tested. The TOC value in the #1 raffinate was 351.2 mg / L, and the TOC value in the #2 raffinate was 289.7 mg / L; the TOC value in the #1 stripping liquid was 283.9 mg / L, and the TOC value in the #2 raffinate was 237.0 mg / L;
[0118] From the above examples, it can be seen that the lithium extraction resin provided by the present invention is used to recover lithium from lithium-containing liquid with almost no solvent loss, while avoiding the environmental problems caused by the volatilization of organic solvents.
[0119] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A lithium extraction resin, characterized in that: It comprises a resin and an ion exchanger distributed in the resin; the ion exchanger is an alkyl salicylate; The lithium extraction resin is in a porous spherical or quasi-spherical shape, and has a particle size of 100 to 200 meshes.
2. The lithium extraction resin according to claim 1, characterized in that The resin is a polystyrene resin; The salicylic acid alkyl ester includes one or more of octyl salicylate, propyl salicylate, butyl salicylate, pentyl salicylate and hexyl salicylate; the mass percentage of the ion exchanger in the lithium extraction resin is 10-60%.
3. The lithium extraction resin according to claim 1, characterized in that The pore volume of the lithium extraction resin is above 2 mL / g, and the specific surface area is 500 m 2 / g or more, and the average pore diameter is more than 10nm.
4. The method for preparing the lithium extraction resin according to any one of claims 1 to 3, characterized in that: The following steps are involved: The monomer, ion exchanger, cross-linking agent, initiator and porogen are first mixed to obtain an organic phase; the ion exchanger is alkyl salicylate; secondly mixing the dispersant, the surfactant and water to obtain an aqueous phase; The organic phase and the aqueous phase are thirdly mixed to obtain a reaction solution; The reaction solution is subjected to a polymerization reaction to obtain the lithium-extracting resin.
5. The preparation method according to claim 4, characterized in that: The monomer is styrene; The cross-linking agent is divinylbenzene; The initiator is benzoyl peroxide, azobisisobutyl cyanide, cumene hydroperoxide or lauroyl peroxide; The porogen is sodium thiocyanate, sodium bicarbonate, sodium carbonate, n-butyl ether or toluene; The dispersant is gelatin or polyvinyl alcohol; The surfactant is sodium dodecyl sulfate or Triton.
6. The preparation method according to claim 4 or 5, characterized in that: The volume ratio of the monomer to the cross-linking agent is 1:0.5-1.5; The volume ratio of the monomer to the reaction liquid is 1:10-20; The mass percentage of the ion exchanger in the organic phase is 10-60%.
7. Use of the lithium extraction resin according to any one of claims 1 to 3 or the lithium extraction resin obtained by the preparation method according to any one of claims 4 to 6 in recovering lithium.
8. A method for recovering lithium from a lithium-containing liquid, characterized in that: The following steps are involved: Passing the lithium-containing feed liquid into a lithium-extracting resin for adsorption to obtain an adsorption tail liquid and a lithium-rich resin; the lithium-extracting resin is the lithium-extracting resin according to any one of claims 1 to 3 or the lithium-extracting resin obtained by the preparation method according to any one of claims 4 to 6; The acid solution is passed into the lithium-rich resin for desorption to obtain a lithium desorption solution.
9. The recycling method according to claim 8, characterized in that: The lithium concentration in the lithium-containing liquid is 0.05 to 10 g / L; the flow rate of the lithium-containing liquid is 2 to 5 BV / h; The ratio of the lithium concentration in the adsorption tail liquid to the lithium concentration in the lithium-containing feed liquid is 1:10-100; the adsorption is stopped when the lithium concentration in the adsorption tail liquid reaches 0.005-1 g / L.
10. The recycling method according to claim 8, characterized in that: The acid solution includes one or more of hydrochloric acid solution, nitric acid solution and sulfuric acid solution; the hydrogen ion concentration of the acid solution is 0.05-6 mol / L; The acid solution is introduced at a flow rate of 0.5 to 2 BV / h.
Citation Information
Patent Citations
Preparation method of low-conductivity diaphragm for lithium-ion battery
CN104300104A
Extraction system and extraction method for extracting lithium from alkaline lithium-containing solution
CN115433830A
Method for selectively extracting lithium from levextrel resin
CN115717200A
Phosphoric acid modified aluminum lithium adsorbent, preparation and method for preparing battery grade lithium carbonate and co-producing potassium chloride from carbonate type salt lake brine
CN115888665A
Preparation method and application of adsorption material for extracting lithium from salt lake
CN116272891A