Metal-doped BNT composite material and preparation method and application thereof

The piezoelectric catalyst prepared by doping metal ions in the BNT matrix solves the problems of slow electron transfer and insufficient active sites in the existing technology, achieves efficient degradation of organic pollutants, and significantly improves the performance and application of the catalyst. prospect.

CN118807728APending Publication Date: 2024-10-22KUNMING UNIV OF SCI & TECH +3
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410788461.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing piezoelectric catalysts have problems with slow electron transfer and insufficient active sites in water treatment, which hinders their application efficiency in removing organic pollutants.

Method used

Using metal-doped BNT composite materials, by doping molybdenum ions, silver ions or copper ions in the BNT matrix, an efficient piezoelectric catalyst is prepared using a solvothermal reaction and calcination process, and an internal electric field is established to suppress electron-hole recombination and improve Redox activity.

Benefits of technology

It achieves efficient degradation of organic pollutants, significantly improves the electronic conductivity and stability of the catalyst, and improves the piezoelectric catalytic degradation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807728A_ABST
    Figure CN118807728A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of piezoelectric catalysis, and particularly relates to a metal-doped BNT composite material and a preparation method and application thereof. The invention provides a metal-doped BNT composite material. The metal-doped BNT composite material comprises a BNT matrix and metal ions doped in the BNT matrix, the chemical composition of the BNT matrix is Bi < 0.5 > Na < 0.5 > TiO < 3 >; the metal ions comprise molybdenum ions, silver ions or copper ions. The metal doped BNT composite material provided by the invention shows ultrahigh piezoelectric catalytic degradation efficiency on organic pollutants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of piezoelectric catalysis, and in particular relates to a metal-doped BNT composite material and a preparation method and application thereof. Background Art

[0002] In recent decades, with the acceleration of urbanization and the development of industrial economy in my country, the discharge of domestic sewage and industrial wastewater has continued to increase, and environmental pollution has become a major problem. Based on the special properties of piezoelectric materials, their piezoelectric catalytic properties are providing strategies for the progress of solving environmental problems.

[0003] Under a certain mechanical pressure, the piezoelectric material is forced to generate positive and negative charges on both sides of the catalyst surface, thereby forming a built-in electric field, separating electrons and holes, and inhibiting the recombination of carriers. Although researchers have made a lot of efforts in the development of piezoelectric catalysts, most piezoelectric catalysts still have problems with slow electron transfer and insufficient active sites, which seriously hinder the application of piezoelectric catalysis in water treatment. Therefore, the development of efficient piezoelectric catalysts is crucial for the piezoelectric catalytic degradation of organic pollutants. Summary of the invention

[0004] The object of the present invention is to provide a metal-doped BNT composite material and a preparation method and application thereof. The metal-doped BNT composite material provided by the present invention has a highly efficient piezoelectric catalytic effect.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a metal-doped BNT composite material, comprising a BNT matrix and metal ions doped in the BNT matrix;

[0007] The chemical composition of the BNT matrix is ​​Bi 0.5 Na 0.5 TiO3;

[0008] The metal ions include molybdenum ions, silver ions or copper ions.

[0009] Preferably, the doping molar percentage of the metal ions is 0-4% based on the molar amount of the metal element, and is not zero.

[0010] The present invention also provides a method for preparing the metal-doped BNT composite material described in the above technical solution, comprising the following steps:

[0011] The BNT matrix, the metal salt and the organic solvent are mixed and subjected to a solvothermal reaction to obtain a precursor material;

[0012] The precursor material is calcined to obtain the metal-doped BNT composite material.

[0013] Preferably, the metal salt includes molybdenum salt, silver salt or copper salt; the organic solvent includes one or more of ethanol, acetone and methanol;

[0014] The amount of the metal salt is 0-4% of the amount of the BNT matrix, and is not zero.

[0015] Preferably, the temperature of the solvent thermal reaction is 50-100° C., and the insulation time is 2-4 hours.

[0016] Preferably, the calcination temperature is 200-300° C., and the holding time is 1-3 hours; the calcination is carried out under a protective atmosphere.

[0017] The present invention also provides the use of the metal-doped BNT composite material described in the above technical solution or the metal-doped BNT composite material prepared by the preparation method described in the above technical solution as a catalyst in degrading organic pollutants.

[0018] Preferably, the application comprises the following steps:

[0019] A solution containing organic pollutants and a catalyst are mixed to perform a piezoelectric catalytic reaction;

[0020] The catalyst is the metal-doped BNT composite material described in the above technical solution or the metal-doped BNT composite material prepared by the preparation method described in the above technical solution.

[0021] Preferably, the concentration of organic pollutants in the solution containing organic pollutants is 10 to 50 mg / L;

[0022] The concentration of the catalyst in the solution containing organic pollutants is 10-50 mg / L.

[0023] Preferably, the piezoelectric catalytic reaction is carried out under ultrasonic conditions, and the frequency of the ultrasound is 37 to 80 KHz.

[0024] The present invention provides a metal-doped BNT composite material, comprising a BNT matrix and metal ions doped in the BNT matrix; the chemical composition of the BNT matrix is ​​Bi 0.5 Na 0.5 TiO3; the metal ions include molybdenum ions, silver ions or copper ions. In the present invention, the piezoelectric material sodium bismuth titanate (Bi 0.5 Na 0.5 TiO3, referred to as BNT) is composed of Na + and Bi 3+The co-occupied perovskite structure ferroelectric is a trigonal system at room temperature and has strong ferroelectric properties. According to the piezoelectric principle, the unit cell of Mo is a body-centered cubic unit cell, while the resistivity of silver and copper is small. Under the same conditions, the "conductor" can be divided into silver and copper according to the conductivity coefficient. The conductivity is better. Therefore, sodium bismuth titanate is used as a matrix to load a certain amount of high-valent Mo, Ag or Cu. Under vibration conditions, it can not only effectively enrich charges and fix electrons, but also has relatively high electronic conductivity. It also has greater catalytic activity and contact sites for organic pollutants. The combination of the two introduces electron traps to enrich active sites, creates a good conductivity and stability environment, and prevents it from recombination with carriers of opposite charge. By adjusting the reaction temperature, Bi with adjustable Mo, Ag, and Cu content was successfully synthesized. 0.5 Na 0.5 TiO3@Mo、Bi 0.5 Na 0.5 TiO3@Ag、Bi 0.5 Na 0.5 TiO3@Cu catalyst was first applied to remove organic pollutants from water by piezoelectric catalysis. The results showed that the composite material provided by the present invention exhibited ultra-high piezoelectric catalytic degradation efficiency for organic pollutants. The ultra-high redox activity was attributed to the establishment of an internal electric field on the surface of the piezoelectric material, and the high-valent Mo, Ag, and Cu species led to the Bi 0.5 Na 0.5 The mobile charge imbalance of TiO3 induces the directional transfer of electrons, effectively inhibits the recombination of electron holes, and enables the redox reaction to proceed effectively. The results confirm that the composite material provided by the present invention has good application prospects in removing pollutants. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Bi obtained in Example 1 0.5 Na 0.5 SEM image of TiO3 piezoelectric material;

[0026] Figure 2 Bi obtained in Example 2 0.5 Na 0.5 SEM image of TiO3@Mo composite piezoelectric material;

[0027] Figure 3 The graph is a graph showing the degradation effect of the composite piezoelectric material obtained in Examples 2 to 5 on organic pollutants;

[0028] Figure 4 This is a diagram showing the CO conversion effect of the composite piezoelectric material obtained in Example 2;

[0029] Figure 5 This is a diagram showing the CO conversion effect of the composite piezoelectric material obtained in Example 5. DETAILED DESCRIPTION

[0030] The present invention provides a metal-doped BNT composite material, comprising a BNT matrix and metal ions doped in the BNT matrix;

[0031] The chemical composition of the BNT matrix is ​​Bi 0.5 Na 0.5 TiO3;

[0032] The metal ions include molybdenum ions, silver ions or copper ions.

[0033] In the present invention, the molar percentage of the metal ions is preferably 0-4% and not 0, based on the molar amount of the metal element.

[0034] The present invention also provides a method for preparing the metal-doped BNT composite material described in the above technical solution, comprising the following steps:

[0035] The BNT matrix, the metal salt and the organic solvent are mixed and subjected to a solvothermal reaction to obtain a precursor material;

[0036] The precursor material is calcined to obtain the metal-doped BNT composite material.

[0037] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0038] The present invention mixes a BNT matrix, a metal salt and an organic solvent, and performs a solvent thermal reaction to obtain a precursor material.

[0039] In the present invention, the BNT matrix is ​​preferably obtained by preparation, and the preparation method preferably includes the following steps: mixing Ti(OC4H9)4, Bi(NO3)3·5H2O, NaOH and water, and performing a hydrothermal reaction to obtain the BNT matrix.

[0040] In the present invention, the dosage ratio of Ti(OC4H9)4 and Bi(NO3)3·5H2O is preferably 5.6mL:3.88g; the mass ratio of Bi(NO3)3·5H2O and NaOH is preferably 3.88:14.4; the dosage ratio of NaOH and water is preferably 14.4g:80mL. In the present invention, the mixing is preferably carried out under the condition of magnetic stirring, and the time of magnetic stirring is preferably 2h. In the present invention, the temperature of the hydrothermal reaction is preferably 160°C, and the time is preferably 24h. After the hydrothermal reaction, the present invention also preferably includes drying the obtained hydrothermal reaction system to obtain the BNT matrix.

[0041] In the present invention, the metal salt preferably includes a molybdenum salt, a silver salt or a copper salt; the molybdenum salt is preferably MoCl5; the silver salt preferably includes silver nitrate; the copper salt preferably includes copper chloride. In the present invention, the organic solvent preferably includes one or more of ethanol, acetone and methanol. In the present invention, the amount of the metal salt preferably accounts for 0 to 4% of the amount of the BNT matrix, and is not 0. In the present invention, the amount ratio of the BNT matrix to the organic solvent is preferably 0.1 g: 20 mL.

[0042] In the present invention, the temperature of the solvothermal reaction is preferably 50 to 100° C., more preferably 60 to 80° C., and the holding time is preferably 2 to 4 hours. In the present invention, the solvothermal reaction is preferably carried out under stirring.

[0043] After obtaining the precursor material, the present invention calcines the precursor material to obtain the metal-doped BNT composite material.

[0044] In the present invention, the calcination temperature is preferably 100-300°C, more preferably 150-250°C, and more preferably 200°C; the holding time is preferably 1-3h; the calcination is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably nitrogen.

[0045] The present invention also provides the use of the metal-doped BNT composite material described in the above technical solution or the metal-doped BNT composite material prepared by the preparation method described in the above technical solution as a catalyst in degrading organic pollutants.

[0046] In the present invention, the application preferably comprises the following steps:

[0047] A solution containing organic pollutants and a catalyst are mixed to perform a piezoelectric catalytic reaction;

[0048] The catalyst is the metal-doped BNT composite material described in the above technical solution or the metal-doped BNT composite material prepared by the preparation method described in the above technical solution.

[0049] In the present invention, the organic pollutants in the solution containing organic pollutants preferably include sulfamethoxazole, enrofloxacin, and tetracycline. In the present invention, the concentration of the organic pollutants in the solution containing organic pollutants is preferably 10 to 50 mg / L; the concentration of the catalyst in the solution containing organic pollutants is preferably 10 to 50 mg / L.

[0050] In the present invention, the piezoelectric catalytic reaction is preferably carried out under ultrasonic conditions, and the frequency of the ultrasound is preferably 37 to 80 KHz.

[0051] In order to further illustrate the present invention, a metal-doped BNT composite material provided by the present invention and its preparation method and application are described in detail below in combination with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0052] Example 1

[0053] First, 5.6 mL of Ti(OC4H9)4, 3.88 g of Bi(NO3)3·5H2O and 14.4 g of NaOH were dissolved in 80 mL of deionized water and stirred magnetically for 2 hours. Then the mixture was poured into a 100 mL autoclave and heated to 160 ° C for 24 hours for hydrothermal reaction. After drying, Bi 0.5 Na 0.5 TiO3 piezoelectric material (BNT);

[0054] Figure 1 Bi obtained in Example 1 0.5 Na 0.5 SEM image of TiO3 piezoelectric material, from Figure 1 You can see the simple Bi 0.5 Na 0.5 Morphology of TiO3.

[0055] Example 2

[0056] 0.1 g of BNT obtained in Example 1 and MoCl5 (wherein the amount of MoCl5 is 3.11% of the molar amount of BNT) are mixed in 20 mL of ethanol to form a suspension; the obtained suspension is stirred at 70° C. for 2 h to perform a solvothermal reaction to obtain a precursor material;

[0057] The obtained precursor material was heated to 300°C in a nitrogen atmosphere for calcination and kept at this temperature for 1 h to obtain Bi 0.5 Na 0.5 TiO3@Mo composite piezoelectric material;

[0058] Figure 2 Bi obtained in Example 2 0.5 Na 0.5 SEM image of TiO3@Mo composite piezoelectric material, Figure 2 It can be seen that the incorporation of molybdenum ions has an important effect on Bi 0.5 Na 0.5 The morphology of TiO3 has not changed much and remains in the shape of nanospheres.

[0059] Example 3

[0060] 0.1 g of BNT obtained in Example 1 and MoCl5 (wherein the amount of MoCl5 is 1.08% of the molar amount of BNT) are mixed in 20 mL of ethanol to form a suspension; the obtained suspension is stirred at 70° C. for 2 h to perform a solvothermal reaction to obtain a precursor material;

[0061] The obtained precursor material was heated to 300°C in a nitrogen atmosphere for calcination and kept at this temperature for 1 h to obtain Bi 0.5 Na 0.5 TiO3@Mo composite piezoelectric materials.

[0062] Example 4

[0063] 0.1 g of BNT obtained in Example 1 and MoCl5 (wherein the amount of MoCl5 is 1.98% of the molar amount of BNT) are mixed in 20 mL of ethanol to form a suspension; the obtained suspension is stirred at 70° C. for 2 h to perform a solvothermal reaction to obtain a precursor material;

[0064] The obtained precursor material was heated to 300°C in a nitrogen atmosphere for calcination and kept at this temperature for 1 h to obtain Bi 0.5 Na 0.5 TiO3@Mo composite piezoelectric materials.

[0065] Example 5

[0066] 0.1 g of BNT obtained in Example 1 and MoCl5 (wherein the amount of MoCl5 is 3.87% of the molar amount of BNT) are mixed in 20 mL of ethanol to form a suspension; the obtained suspension is stirred at 70° C. for 2 h to perform a solvothermal reaction to obtain a precursor material;

[0067] The obtained precursor material was heated to 300°C in a nitrogen atmosphere for calcination and kept at this temperature for 1 h to obtain Bi 0.5 Na 0.5 TiO3@Mo composite piezoelectric materials.

[0068] Performance Testing

[0069] The Bi obtained in Examples 2 to 5 0.5 Na 0.5 The catalytic performance of TiO3@Mo composite piezoelectric material was tested;

[0070] An aqueous solution containing organic pollutants and a composite piezoelectric material were mixed (wherein the organic pollutant was sulfamethoxazole, and the concentration of the organic pollutant was 50 mg / L; the concentration of the composite piezoelectric material was 30 mg / L), and the piezoelectric degradation effect was studied under the conditions of no ultrasound, a frequency of 37HKz, and a frequency of 80KHz, respectively. The test results are shown in Table 1, Table 2, and Table 3, respectively;

[0071] Table 1 Degradation effect without ultrasound

[0072]

[0073] Table 2 Degradation effect under ultrasonic 37KHz condition

[0074]

[0075]

[0076] Table 3 Degradation effect under ultrasonic 80KHz condition

[0077]

[0078] Figure 3 The degradation effect diagram is shown in Figure 2. Figure 3 It can be seen that the composite catalyst Bi 0.5 Na 0.5 TiO3@Mo (3.87%) has the best degradation effect on sulfamethoxazole at 37KHz.

[0079] Figure 4 Bi obtained in Example 2 0.5 Na 0.5 CO conversion effect diagram of TiO3@Mo (3.11%) composite piezoelectric material, from Figure 4 It can be seen that sulfamethoxazole is degraded and converted into CO2 (515.8ppm), and CO2 is further piezoelectrically reduced to usable energy CO (15.6ppm).

[0080] Figure 5 Bi obtained in Example 5 0.5 Na 0.5 CO conversion effect diagram of TiO3@Mo (3.87%) composite piezoelectric material, from Figure 5 It can be seen that sulfamethoxazole is degraded and converted into CO2 (715.8ppm), and CO2 is further piezoelectrically reduced to usable energy CO (22.6ppm)

[0081] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A metal-doped BNT composite material, characterized in that: comprising a BNT matrix and metal ions doped in the BNT matrix; The chemical composition of the BNT matrix is ​​Bi 0.5 Na 0.5 TiO3; The metal ions include molybdenum ions, silver ions or copper ions.

2. The metal-doped BNT composite material according to claim 1, characterized in that: Calculated on the molar amount of the metal element, the doping molar percentage of the metal ion is 0-4%, and is not 0.

3. The method for preparing the metal-doped BNT composite material according to any one of claims 1 to 2, characterized in that: The following steps are involved: The BNT matrix, the metal salt and the organic solvent are mixed and subjected to a solvothermal reaction to obtain a precursor material; The precursor material is calcined to obtain the metal-doped BNT composite material.

4. The preparation method according to claim 3, characterized in that: The metal salt includes molybdenum salt, silver salt or copper salt; the organic solvent includes one or more of ethanol, acetone and methanol; The amount of the metal salt is 0-4% of the amount of the BNT matrix, and is not zero.

5. The preparation method according to claim 3, characterized in that: The temperature of the solvent thermal reaction is 50-100° C., and the insulation time is 2-4 hours.

6. The preparation method according to claim 3, characterized in that: The calcination temperature is 100-300° C., and the heat preservation time is 1-3 hours; the calcination is carried out under a protective atmosphere.

7. Use of the metal-doped BNT composite material according to any one of claims 1 to 2 or the metal-doped BNT composite material prepared by the preparation method according to any one of claims 3 to 6 as a catalyst in degrading organic pollutants.

8. The use according to claim 7, characterized in that: The application comprises the following steps: A solution containing organic pollutants and a catalyst are mixed to perform a piezoelectric catalytic reaction; The catalyst is the metal-doped BNT composite material according to any one of claims 1 to 2 or the metal-doped BNT composite material prepared by the preparation method according to any one of claims 3 to 6.

9. The use according to claim 8, characterized in that: The concentration of organic pollutants in the solution containing organic pollutants is 10 to 50 mg / L; The concentration of the catalyst in the solution containing organic pollutants is 10-50 mg / L.

10. The use according to claim 8, characterized in that: The piezoelectric catalytic reaction is carried out under ultrasonic conditions, and the frequency of the ultrasound is 37-80 KHz.

Citation Information

Patent Citations

  • Preparation method of adsorption type piezoelectric photocatalytic composite fiber material

    CN113385213A

  • Bismuth layer structure piezoelectric heterojunction catalyst and preparation method thereof

    CN114602482A