Machining method for TB9 titanium alloy cylindrical helical compression spring

Through the optimization of TB9 titanium alloy materials and process parameters, the length attenuation and stress relaxation problems of cylindrical spiral compression springs are solved, corrosion resistance and lightweight effects are achieved, and the needs of the aerospace field are met.

CN118809094AActive Publication Date: 2024-10-22XIAN KUNLUN IND GRP

Patent Information

Application Number
CN202411029132.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-22
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Existing cylindrical spiral compression springs suffer from length attenuation and stress relaxation during use, are prone to rust, and cannot meet the lightweight requirements in the aerospace field.

Method used

The cylindrical spiral compression spring is processed from TB9 titanium alloy material. By controlling the temperature, time and exit temperature of the aging treatment, the tensile strength is ensured between 1300MPa and 1350MPa. The process parameters are adjusted to meet the spring's requirements by combining shot peening and dynamic fatigue testing. life requirements.

Benefits of technology

It achieves the effects of small stress relaxation resistance and small length attenuation, while meeting corrosion resistance and lightweight requirements, and improving the service life and performance consistency of the spring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118809094A_ABST
    Figure CN118809094A_ABST
Patent Text Reader

Abstract

The invention provides a TB9 titanium alloy cylindrical helical compression spring machining method. The TB9 titanium alloy cylindrical helical compression spring machining method comprises the steps that a solid-solution-state TB9 titanium alloy wire is adopted for material preparation; the wire is wound into a cylindrical helical compression spring body; grinding two end surfaces of the spring; the spring is subjected to aging treatment, so that the tensile strength is between 1,300 MPa and 1,350 MPa; a spring is arranged on the mandrel in a penetrating mode, the spring is extruded to be in a pressed state, and the state is kept for preset time; and a dynamic fatigue test is carried out after shot blasting treatment, whether the length and the load of the spring meet the requirements of not smaller than specified values or not is judged, and if the current batch of products are unqualified, the aging treatment temperature, time and tapping temperature of the next batch of parts are adjusted till the parts meet the service life requirements. According to the method, the cylindrical helical compression spring is obtained through a simple technological process, the free length and rigidity of the spring are hardly attenuated and relaxed within the service life, the purposes of stress relaxation resistance and attenuation resistance are achieved, and meanwhile the TB9 titanium alloy material can meet the requirements for corrosion resistance and light weight.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of spring processing, and specifically relates to a processing method of a TB9 titanium alloy cylindrical helical compression spring. Background Art

[0002] As a mechanical part, springs need to frequently bear complex loads, perform reciprocating deformation and reset motions during use to play the role of buffering and shock absorption. In particular, buffer springs and firing springs have complex use environments, high movement frequencies, and long service life. Springs must have a high fatigue life and a certain degree of corrosion resistance. If used in the fields of aviation and aerospace, lightweighting is also a factor that must be considered.

[0003] Cylindrical helical compression springs are the most common type of springs. Currently, they are mainly made of carbon spring steel wire, alloy spring steel wire and stainless steel spring steel wire. However, springs made of these materials will experience length attenuation and stress relaxation during use, which affects the life of the springs. They are also prone to rust and cannot meet the lightweight requirements of the aerospace field. Summary of the invention

[0004] In order to solve the problems that existing cylindrical helical compression springs have length attenuation and stress relaxation during use, are prone to rust, and cannot meet the lightweight requirements, the present invention proposes a TB9 titanium alloy cylindrical helical compression spring processing method, aiming to provide a spring with low stress relaxation resistance, low length attenuation, and which meets the corrosion resistance and lightweight requirements.

[0005] The inventive concept of the present invention:

[0006] First of all, the present invention proposes to use TB9 titanium alloy to process cylindrical helical compression springs, which can achieve the expected weight reduction effect. Compared with springs of the same specifications, the weight can be reduced by 42.55%. In addition, TB9 titanium alloy material has strong corrosion resistance. Compared with carbon spring steel wire and alloy spring steel wire, titanium alloy springs do not require surface anti-corrosion treatment and can meet general use requirements by relying on the material's own anti-corrosion properties.

[0007] Furthermore, the applicant found during the test that the cylindrical helical compression spring made of TB9 titanium alloy was prone to failure to meet the test parameters and product batch failure in fatigue tests. Through a lot of analysis and research, the applicant found that the tensile strength of the spring was too high after aging treatment, too close to the limit value of 1400MPa, resulting in a poor life of the produced spring. In response to this problem, the applicant considered controlling the temperature, time and furnace temperature of the aging treatment during the heat treatment process, so that the tensile strength of the obtained spring is not too close to the limit value, to ensure that the parameters of the final processed spring meet the requirements and improve the life of the spring.

[0008] To achieve the above purpose, the technical solution provided by the present invention is:

[0009] A method for processing a TB9 titanium alloy cylindrical helical compression spring comprises the following steps:

[0010] Step 1, material preparation: using solid solution TB9 titanium alloy wire material for material preparation;

[0011] Step 2, spring winding: winding the wire into a spring body of a cylindrical helical compression spring;

[0012] Step 3, grinding the end faces: Grind the two end faces of each spring;

[0013] Step 4, aging treatment: put the spring into a vacuum heat treatment furnace, age it at a preset temperature for a predetermined time, and take it out of the furnace after cooling, so that the tensile strength of the spring is between 1300MPa and 1350MPa;

[0014] Step 5, strong pressure treatment: put the spring on the mandrel, squeeze the spring to make it in a compressed state, and keep it for a predetermined time;

[0015] Step 6, shot peening: Use steel shot smaller than 1 / 2 of the wire diameter to shot peen the spring, and the shot peening coverage is required to be more than 90%;

[0016] Step 7, dynamic fatigue test: randomly select 3% of the springs, load the springs with periodic loads, stop the machine after a predetermined number of cycles and detect the length and load of the springs; determine whether the length and load of the springs meet the requirement of not less than the specified value. If one spring part does not meet the requirement, double the number of parts will be selected and retested. If there are still parts that do not meet the requirements after the retest, the current batch of products is determined to be unqualified, and the aging treatment temperature, time and furnace temperature of the next batch of parts will be adjusted in step 4 until the parts meet the requirements.

[0017] Furthermore, in step 2, an automatic spring winding machine is used to wind the spring body.

[0018] Furthermore, in step 2, the spring body is wound by using a lathe core winding method.

[0019] Furthermore, in step 3, a spring grinding machine is used to grind the spring end surface.

[0020] Further, in step 3, the spring end surface is manually ground using a grinding machine.

[0021] Furthermore, in step 3, when the grinding amount is too large, the two end surfaces of the spring body are first cut by wire cutting and then fine-grinded.

[0022] The advantages of the present invention are:

[0023] 1. The TB9 titanium alloy cylindrical helical compression spring processing method of the present invention adopts solid solution TB9 titanium alloy wire to manufacture cylindrical helical compression springs. After the spring body is wound and formed, the spring end surface is ground and then heat treated. During the aging treatment, the tensile strength is controlled not to be too close to the limit value, between 1300MPa and 1350MPa. Finally, a dynamic fatigue test is performed to check whether the spring life is qualified. If it is unqualified, the temperature and time of the aging treatment are adjusted to make the parts meet the life requirements. In this way, a cylindrical helical compression spring can be obtained with a simple process flow, and the free length and stiffness of the spring are almost not attenuated and relaxed within the service life, thereby achieving the purpose of resisting stress relaxation and attenuation. At the same time, the TB9 titanium alloy material can meet the requirements of corrosion resistance and lightweight.

[0024] 2. The spring winding and end surface grinding processes in the present invention can select alternative solutions for large-scale and small-batch production modes, and the process applicability is strong. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The above and / or other features and advantages of the present invention will become more easily understood through the following description with reference to the accompanying drawings, which are not drawn to scale and some features are exaggerated or reduced to show details of specific components. In the accompanying drawings:

[0026] Figure 1 It is a flow chart of the method for processing a TB9 titanium alloy cylindrical helical compression spring of the present invention;

[0027] Figure 2 It is a schematic diagram of the parts obtained in the example of the present invention;

[0028] Figure 3 It is a fracture failure picture of a part obtained in an example of the present invention after a fatigue test;

[0029] Figure 4 It is a fracture picture of the part obtained in the example of the present invention. DETAILED DESCRIPTION

[0030] The present invention will be described in detail below with reference to the accompanying drawings by means of exemplary embodiments of the present invention. It should be noted that the following detailed description of the present invention is only for the purpose of illustration, and is not intended to limit the present invention.

[0031] The present invention provides a method for processing a TB9 titanium alloy cylindrical helical compression spring, which is used to provide a method for processing a cylindrical helical compression spring using TB9 titanium alloy material, and can obtain a spring with low stress relaxation resistance and low length attenuation, while meeting the requirements of corrosion resistance and lightweight.

[0032] Reference Figure 1As an exemplary embodiment of the present invention, a method for processing a TB9 titanium alloy cylindrical helical compression spring may include the following steps:

[0033] Step S1, material preparation: using solid solution TB9 titanium alloy wire material for material preparation;

[0034] Step S2, spring winding: winding the wire into a spring body of a cylindrical helical compression spring;

[0035] Step S3, grinding the end surfaces: grinding the two end surfaces of each spring;

[0036] Step S4, aging treatment: placing the spring into a vacuum heat treatment furnace, aging the spring at a preset temperature for a predetermined time, and taking the spring out of the furnace after cooling, so that the tensile strength of the spring is between 1300MPa and 1350MPa;

[0037] Step S5, strong pressing treatment: putting the spring on the mandrel, squeezing the spring to make it in a compressed state, and keeping it for a predetermined time;

[0038] Step S6, shot peening: using steel shot smaller than 1 / 2 of the wire diameter to shot peen the spring, requiring the shot peening coverage to be more than 90%;

[0039] Step S7, dynamic fatigue test: randomly select 3% of the springs, load the springs with periodic loads, stop the machine after a predetermined number of cycles and detect the length and load of the springs; determine whether the length and load of the springs meet the requirement of not less than the specified value. If one spring part does not meet the requirement, double the number of parts are selected and retested. If there are still parts that do not meet the requirements after the retest, the current batch of products is determined to be unqualified, and the temperature, time and furnace temperature of the aging treatment of the next batch of parts are adjusted in step S4 until the parts meet the requirements.

[0040] In step S1, TB9 titanium alloy wire is used. The material has the advantages of good corrosion resistance, high fatigue life, and low density. The density is 4.51g / cm3, which is 57.45% of the density of common steel. The wire is in a solid solution state and has good processing technology. The solid solution treatment process after spring forming can be avoided to avoid deformation of the spring during solid solution treatment.

[0041] In the spring winding process of step S2, automatic spring winding machines are preferably used for winding, which have the advantages of high production efficiency, good product consistency, and are suitable for mass production. When the production batch is small, in order to save materials, lathe core winding can be used for winding.

[0042] In step S3, a spring grinding machine is preferably used to grind the end faces. The advantages are good parallelism and verticality of the two end faces, high production efficiency, good product consistency, and suitability for mass production. When the production batch is small or there is no automatic spring winding machine, in order to save costs, a grinding wheel machine can be used instead of a spring grinding machine for manual grinding.

[0043] In addition, when the grinding amount is too large, wire cutting can be used for rough cutting first, and then fine grinding can be performed to achieve the required size. The heat-affected surface of wire cutting must be ground off to eliminate the hidden danger of micro-cracks caused by wire cutting.

[0044] The aging treatment in step S4 must be carried out after grinding the end surface, which can eliminate the stress caused by grinding. Through aging treatment, the strength of the spring material can be controlled within a certain range, so that the spring can reach the longest life. A vacuum heat treatment furnace is used to age the spring at a specific temperature for a certain period of time. After leaving the furnace, the tensile strength of the material is between 1300MPa and 1350MPa, the surface gloss of the spring is good, there is no obvious oxidation or discoloration, and it is not too close to the strength limit of 1400MPa, so as to ensure that the parts meet the detection requirements in the final fatigue test.

[0045] In step S5, the strong pressure treatment is to reduce stress concentration and effectively increase the life of the spring.

[0046] Before shot peening in step S6, the spring must not be stressed or deformed, otherwise the spring will be irreversibly deformed after the shot peening. Shot peening can eliminate defects such as microcracks on the surface of the material and reduce stress concentration. On the other hand, it can produce a new stress layer on the surface of the material to achieve the purpose of applying prestress, which can effectively offset the load on the spring during use. Shot peening can significantly increase the service life of the spring.

[0047] Step S7 is to verify whether the service life of the processed parts meets the requirements. After loading the spring with a certain conditional periodic load, the length and load of the spring are tested, that is, the length attenuation and stress relaxation are verified, and then the test parameters are determined to be not less than the specified value. For a batch, if one part of 3% of the springs breaks or does not meet the requirements during the experiment, the parts are doubled and tested again. If there are still parts that do not meet the requirements, the batch of products is considered unqualified. In this case, for the next batch of parts, the treatment temperature and time need to be adjusted during the aging treatment to ensure that the spring life meets the requirements.

[0048] As described above, the present invention can obtain a cylindrical helical compression spring with a simple process flow, and the free length and stiffness of the spring will hardly decay and relax during its service life, achieving the purpose of anti-stress relaxation and anti-decay, and at the same time, the TB9 titanium alloy material can meet the requirements of corrosion resistance and lightweight. In addition, the spring winding and end face grinding process in the present invention can select alternative solutions for large-scale and small-scale production modes, and the process applicability is strong.

[0049] Next, the processing method of the TB9 titanium alloy cylindrical helical compression spring provided by the present invention is further described with reference to examples.

[0050] In this example, if Figure 2As shown, the dimensions of the spring parts to be processed are: spring center diameter D = 9.23mm, titanium alloy wire diameter d = Φ2.27mm, spring pitch t = 4.69mm, spring free length H 0 =55±1mm, spring preload length H 1 =46mm, spring working length H 2 =34mm, spring compression height H b =30.8mm, spring load F 1 =140±10N, spring load F 2 =328±20N, spring load F when compressed b =376.4N, total number of spring turns n1 = 13 ± 0.75 turns, effective turns n = 11 turns.

[0051] The processing process is as follows:

[0052] Process 1, material preparation: TB9 solid solution titanium wire with a size of Φ2.27mm is used, and the whole reel is prepared. The material passes the on-site re-inspection and the actual wire diameter is Φ2.29mm, which meets the tolerance requirements.

[0053] Process 2, spring winding: 1A62 lathe is used for core winding, the core rod diameter is Φ6.4, and the pitch is reserved for deformation after compression. The total number of turns after the spring is cut into single pieces by the lathe is n1 = 13 to 13.15 turns.

[0054] Process 3, grinding the end face: Use a grinding machine to manually grind the end face, support the end face with 3 / 4 circle, and grind the end face with spring H 0 Allow for deformation after compression.

[0055] Step 4, aging treatment: Aging heat treatment is carried out in a vacuum heat treatment furnace at 500°C for 5 hours, and the sample is taken out of the furnace when it cools to 100°C. After being taken out of the furnace, the sample is tested and the tensile strength σ b =1320Mpa, yield strength σ s =1215Mpa.

[0056] Step 5, strong pressure treatment: put the spring on the Φ6.4 mandrel and press it to Hb and keep it for 24 hours.

[0057] Process 6, shot peening: Use 1mm steel shot and current 39A for 10 minutes of rolling shot peening, and the shot peening coverage rate is more than 95%.

[0058] Process 7, parts inspection: Randomly select 2 pieces from the finished parts for inspection. The product dimensions meet the requirements of the drawings, as follows:

[0059] Part Number Length H0 Diameter D1 Load P2 ① 54.5 11.51 330 ② 54.7 11.51 332

[0060] Process 8, fatigue test: Fatigue test is performed on the above two parts. Test conditions: frequency 710 times / min, amplitude H 1 ~H 2 , room temperature, mandrel Φ6.3, the test cycle was 100000 times and then stopped, the length of the spring was attenuated, that is, the length of the spring expanded H 0 The change of stress relaxation, that is, the spring load P2, is tested until the spring fatigue breaks. The spring fracture failure and fracture conditions are as follows: Figure 3 and Figure 4 The test data is as follows:

[0061]

[0062] The results in the above table show that the parts produced by the TB9 titanium alloy cylindrical helical compression spring processing method of the present invention meet the requirements of the drawings and the process is feasible. Fatigue tests have shown that the length and stiffness of the TB9 titanium alloy spring reach a stable state within 30 minutes under the test environment, and the length and stiffness remain unchanged within 60 minutes after stabilization, that is, the anti-stress relaxation and length attenuation effects are obvious.

[0063] Finally, it should be noted that the features mentioned and / or shown in the above description of the exemplary embodiments of the present invention may be combined in the same or similar manner into one or more other embodiments, combined with the features in other embodiments or substituted for the corresponding features in other implementations. The technical solutions obtained by these combinations or substitutions shall also be deemed to be included in the protection scope of the present invention.

Claims

1. A method for processing a TB9 titanium alloy cylindrical helical compression spring, characterized in that: The following steps are involved: Step 1, material preparation: using solid solution TB9 titanium alloy wire material for material preparation; Step 2, spring winding: winding the wire into a spring body of a cylindrical helical compression spring; Step 3, grinding the end faces: Grind the two end faces of each spring; Step 4, aging treatment: put the spring into a vacuum heat treatment furnace, age it at a preset temperature for a predetermined time, and take it out of the furnace after cooling, so that the tensile strength of the spring is between 1300MPa and 1350MPa; Step 5, strong pressure treatment: put the spring on the mandrel, squeeze the spring to make it in a compressed state, and keep it for a predetermined time; Step 6, shot peening: Use steel shot smaller than 1 / 2 of the wire diameter to shot peen the spring, and the shot peening coverage is required to be more than 90%; Step 7, dynamic fatigue test: randomly select 3% of the springs, load the springs with periodic loads, stop the machine after a predetermined number of cycles and detect the length and load of the springs; determine whether the length and load of the springs meet the requirement of not less than the specified value. If one spring part does not meet the requirement, double the number of parts are selected and retested. If there are still parts that do not meet the requirements after the retest, the current batch of products is determined to be unqualified, and the aging treatment temperature, time and furnace temperature of the next batch of parts are adjusted in step 4 until the parts meet the requirements.

2. The method for processing a TB9 titanium alloy cylindrical helical compression spring according to claim 1, characterized in that: In step 2, an automatic spring winding machine is used to wind the spring body.

3. The method for processing a TB9 titanium alloy cylindrical helical compression spring according to claim 1, characterized in that: In step 2, the spring body is wound by core winding on a lathe.

4. The method for processing a TB9 titanium alloy cylindrical helical compression spring according to claim 1 or 2, characterized in that: In step 3, a spring grinding machine is used to grind the spring end surface.

5. The method for processing a TB9 titanium alloy cylindrical helical compression spring according to claim 1 or 2, characterized in that: In step 3, the spring end surface is manually ground using a grinding machine.

6. The method for processing a TB9 titanium alloy cylindrical helical compression spring according to claim 1 or 2, characterized in that: In step 3, when the grinding amount is too large, the two end faces of the spring body are first cut by wire cutting and then fine-grinded.

Citation Information

Patent Citations

  • Titanium alloy for spring parts and preparation method of alloy

    CN102936673A

  • Preparation method of titanium alloy spring made of wire with specially-shaped section

    CN104174791A

  • High temperature spring processing technology

    CN104607880A

  • Lightweight design method for high-precision large-specification TB9 alloy cylindrical helical compression spring

    CN116484546A

  • Titanium alloy member and manufacturing method therefor

    JP2006022402A

Cited By

  • Forming process of titanium alloy cylindrical spiral spring for aerospace craft

    CN120830066A

  • Forming process of titanium alloy cylindrical coil spring for aerospace vehicle

    CN120830066B