Method for strengthening surface of aviation tenon structure

Through ultrasonic shot peening and deep-cool auxiliary technology, the problems of low surface hardness and poor stability of the aerial tenon structure are solved, and the effect of improving wear and fatigue resistance is achieved, forming an efficient aerial tenon structure strengthening method.

CN118932151APending Publication Date: 2024-11-12CENT SOUTH UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411114477.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The aerial tenon structure is prone to micro-moving wear and micro-moving fatigue during the working process. The existing shot peening strengthening process has problems such as low surface hardness, low residual compressive stress, loose stress and poor stability, especially in the turbine disc tongue and groove area. Complex structure and size limitations lead to uneven reinforcement.

Method used

The ultrasonic strengthening system and deep-cooling device are used to shoot peer the surface of the aeronautical tenon structure. The ultrasonic high-frequency vibration excitation pellets impact the surface produce superstrain plastic deformation and dislocation. The deep-cooling assists in suppressing the dynamic resumption of dislocations and promoting twinning. The nuclear and martensite phase transitions to form nanofine crystals, which improves surface hardness and residual compressive stress.

Benefits of technology

It significantly improves the wear resistance and fatigue resistance of the surface of the aerial tenon structure, solves the surface hardness and stability problems, and provides an effective strengthening method for the aerial tenon structure under severe working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932151A_ABST
    Figure CN118932151A_ABST
Patent Text Reader

Abstract

The invention discloses a strengthening method for the surface of an aviation tenon structure. Shot peening strengthening is conducted on the surface of the tenon structure through an ultrasonic strengthening system, and meanwhile auxiliary strengthening is conducted through a cryogenic device. The ultrasonic strengthening system comprises a tenon strengthening system and a mortise strengthening system, the tenon adopts an integral strengthening mode, and the mortise adopts a single-groove strengthening mode; under the excitation of ultrasonic high-frequency vibration, the pellets impact the surface of the tenon structure at high frequency, so that the surface of the tenon structure is promoted to generate plastic deformation with overstrain, dislocation, twin crystals, sub-crystals and the like, grain refinement is realized, the surface hardness of the tenon structure is improved, and high residual compressive stress is implanted; the cryogenic assistance can improve the plastic flow stress of the metal, is beneficial to inhibiting dislocation dynamic recovery and cross slippage, promoting twin crystal nucleation, improving the martensite phase transformation probability, forming nano fine grains, improving the stability of the strengthened structure, and further improving the surface hardness and residual compressive stress. The method can solve the problems of low surface hardness, low residual compressive stress, stress relaxation, poor stability and the like of the aviation tenon structure subjected to shot peening strengthening in the prior art, improves the wear resistance and fatigue resistance of the surface of the aviation tenon structure, and provides a way for surface strengthening of the aviation tenon structure under severe working conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal surface strengthening and relates to a method for strengthening the surface of an aviation tenon structure. Background Art

[0002] As the power source of an aircraft, the aircraft engine is known as the "heart" of the aircraft. Its good and stable operating condition is a key factor in ensuring the safety of civil aircraft and the performance of fighter jets. In aircraft engines, the blades and the impeller are often connected by a tenon structure. During the operation of the aircraft engine, the tenon structure (tenon and mortise) connection is affected by centrifugal force and strong aerodynamic loads. Normal stress exists on the contact surface, and a small amount of relative sliding occurs. There is a relatively serious risk of micro-motion wear and micro-motion fatigue. Therefore, strengthening the surface of the aircraft tenon structure and improving its wear resistance and fatigue resistance are of great significance to the reliability and service life of the aircraft engine.

[0003] CN201810754114.3 discloses a composite strengthening method for a thin-walled wheel disc, which uses pneumatic shot peening to strengthen the turbine disc, and adopts different shot peening strengthening parameters for different positions of the turbine disc. The space of the wheel disc mortise and tenon area is small, the structure is complex, and it has characteristic structures such as grooves and shielding. In addition, due to the size requirements, the pneumatic shot peening surface strengthening process is prone to cause problems such as shot accumulation, high roughness, and uneven surface strengthening, which in turn leads to uneven stress distribution in the strengthened area of ​​the mortise and tenon, and easy to deform beyond the tolerance. In addition, compressed air is used as the impact energy, and the process controllability is poor. After each shot peening, the projectiles need to be collected, cleaned, and broken and removed, which causes great pollution to the working environment. Summary of the Invention

[0004] The object of the present invention is to provide a strengthening method capable of improving the densification and stability of the surface microstructure of an aviation tenon structure.

[0005] The method for strengthening the surface of an aviation tenon structure provided by the present invention performs shot peening strengthening on the tenon structure surface through an ultrasonic strengthening system and simultaneously performs auxiliary strengthening through a deep cooling device; the ultrasonic strengthening system includes a tenon strengthening system and a tenon groove strengthening system, the tenon adopts an overall strengthening method, and the tenon groove adopts a single groove strengthening method; under the excitation of ultrasonic high-frequency vibration, the pellets impact the tenon structure surface at a high frequency, promoting superstrain plastic deformation on the tenon structure surface, generating dislocations, twins, subgrains, etc., achieving grain refinement, improving the surface hardness of the tenon structure, and implanting high residual compressive stress; deep cooling assistance can increase the plastic flow stress of the metal, which is beneficial to inhibiting the dynamic recovery and cross slip of dislocations, promoting twin nucleation, increasing the probability of martensitic phase transformation, forming nano-fine crystals, improving the stability of the strengthened structure, and further improving the surface hardness and residual compressive stress.

[0006] When the above method is implemented, the tenon strengthening system includes a workbench, an ultrasonic vibration system, a shot peening chamber and a tenon driving device. The shot peening chamber and the ultrasonic vibration system are both fixed on the workbench. The vibration head connected to the upper end of the amplitude rod of the ultrasonic vibration system extends into the bottom of the shot peening chamber. The rotary actuator of the tenon driving device extends horizontally into the shot peening chamber above the corresponding vibration head, and the end is connected to a clamp for installing the tenon.

[0007] When the above method is implemented, the shot blasting chamber includes a cylinder and a base and a top cover connected at both ends thereof. The outer diameter of the base matches the inner diameter of the cylinder, and the top cover is an elliptical cover. The gap between the vibrating head and the base is matched, and the matching gap is smaller than the diameter of the shot.

[0008] When the above method is implemented, the tenon drive device includes a motor, a coupling and the clamp. The motor is arranged with its output shaft in a horizontal direction, and the output shaft and the clamp are connected by a coupling to form the rotary actuator.

[0009] When the above method is implemented, the mortise and tenon strengthening system includes a workbench, a turbine disc drive device, a combined module slide and an ultrasonic vibration system; the turbine disc drive device adopts a horizontal rotary platform, which is fixed on the workbench; the combined module slide includes a horizontal module slide and a vertical module slide connected to its slider, and the horizontal module slide is fixed on the side of the workbench corresponding to the horizontal rotary platform; the transducer and amplitude rod of the ultrasonic vibration system are arranged horizontally, connected to the slider of the vertical module slide through a horizontal bracket, and the vibration head connected to the amplitude rod is inserted into the mortise and tenon.

[0010] When the above method is implemented, the mortise and tenon strengthening system includes a workbench, a turbine disc drive device, a vertical module slide, a horizontal module slide and an ultrasonic vibration system; the vertical module slide is fixed on the workbench, the turbine disc drive device adopts a vertical turntable, and the vertical turntable is connected to the slider of the vertical module slide; the horizontal module slide is fixed on the workbench, the transducer and the amplitude rod of the ultrasonic vibration system are arranged vertically, and are connected to the slider of the horizontal module slide through a combined bracket, and the vibration head connected to the amplitude rod is inserted into the mortise and tenon.

[0011] When the above method is implemented, an auxiliary bracket is provided on the rear side of the workbench corresponding to the vertical module slide, and a clamping plate for connecting the auxiliary bracket is provided on the rear side of the vertical module slide.

[0012] When the above method is implemented, the tongue and groove strengthening system also includes a shot circulation device, which includes a shot storage box and a shot blasting pipe and a recovery pipe connected thereto. The shot blasting pipe is connected to a shot conveying pump, the end of the shot blasting pipe is connected to a shot blasting gun, and the end of the recovery pipe is connected to a cone bucket. The shot blasting gun is located directly above the vibration head, and the cone bucket is fixed on the workbench in the area below the corresponding vibration head, and a corresponding hole is opened on the workbench at the corresponding cone bucket.

[0013] When the above method is implemented, the shape of the vibration head matches the mortise and tenon, and the assembly gap is 2-10 mm.

[0014] When the above method is implemented, the cryogenic device includes a liquid nitrogen bottle and a nitrogen delivery pipeline connected thereto.

[0015] This invention uses ultrasonic shot peening and cryogenic cooling to form nano-fine crystals in the surface material of the tenon-groove structure, increasing surface hardness and instilling high residual compressive stress, thereby improving the wear and fatigue resistance of the tenon structure. This approach addresses the challenges of existing shot peening methods for aviation tenon structures, such as low surface hardness, low residual compressive stress, stress relaxation, and poor stability. It improves the wear and fatigue resistance of aviation tenon structures, providing a solution for strengthening aviation tenon surfaces under harsh operating conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is an axonometric diagram of embodiment 1 of the present invention.

[0017] Figure 2 for Figure 1 An enlarged schematic diagram of the assembly of the middle shot peening cavity and the tenon drive device.

[0018] Figure 3 This is a front view structural diagram of embodiment 2 of the present invention.

[0019] Figure 4 for Figure 3 Schematic diagram of the top view structure.

[0020] Figure 5 for Figure 3 Axonometric structural diagram.

[0021] Figure 6 This is a front view structural diagram of embodiment 3 of the present invention.

[0022] Figure 7 for Figure 6 Axonometric structural diagram. DETAILED DESCRIPTION

[0023] Example 1: This example strengthens the surface of the blade tenon of the aviation tenon structure.

[0024] Combine Figure 1-2 It can be seen that the tenon strengthening system in this embodiment includes a workbench A, an ultrasonic vibration system B, a shot blasting chamber C, and a tenon driving device D. The tenon strengthening system is equipped with a cryogenic device E.

[0025] The upper end of the transducer B2 of the ultrasonic vibration system B is connected to the amplitude transformer B3, and the upper end of the amplitude transformer is connected to the vibration head. The vibration head is a cylindrical structure with a protective cover B4 on the outer wall. A flange is fixed below the protective cover, and the flange is connected to a circle of pull rods B5.

[0026] The shot blasting chamber C includes a cylindrical body C1 and a base C2 and a top cover C3 connected at both ends thereof.

[0027] The base C2 is a hollow inverted T-shape, and the top is welded to the bottom of the cylinder C1.

[0028] The top cover C3 is an elliptical cover and is assembled with the cylindrical body C1 through a tongue-and-groove joint.

[0029] The tenon driving device D includes a servo motor D1, an expansion clamp D2 and a coupling D3. The motor is arranged with its output shaft in the horizontal direction. The expansion clamp is used to clamp the tenon ST of the workpiece to be strengthened.

[0030] The cryogenic device E includes a liquid nitrogen bottle E1 and a nitrogen delivery pipeline connected thereto. The nitrogen delivery pipeline includes a delivery pipe and a pressure gauge E2 connected to its inlet end and a one-way throttle valve E3 connected to its outlet end.

[0031] The assembly process of the tenon reinforcement system is as follows:

[0032] The base C2 of the shot blasting chamber C is placed on the mounting plate of the workbench A, and a through circular hole is opened at the position of the workbench corresponding to the shot blasting chamber.

[0033] The ultrasonic generator B1 of the ultrasonic vibration system B is placed on the mounting plate of the workbench A. The top of the vibration head is inserted into the base of the shot peening chamber C. The installation gap between the outer wall of the vibration head and the inner wall of the base is smaller than the selected shot peening pellet diameter. The upper end of the pull rod B5 passes through the bottom plate of the base C2 and is locked by a nut.

[0034] The selected shot peening pellets are placed on the vibration head of the ultrasonic vibration system B.

[0035] The motor D1 of the tenon drive device D is fixed to the mounting plate of the workbench A through a support. The bulging fixture D2 extends into the cylinder C1 of the shot blasting chamber above the corresponding vibration head, and the mounting hole on the cylinder is sealed.

[0036] Remove the top cover C3 of the shot blasting chamber C, install the blade tenon ST to be strengthened on the bulging fixture D2 and Figure 2 to the position shown, and then reinstall the top cover.

[0037] Finally, the outlet pipe of the one-way throttle valve E3 of the cryogenic device E is connected to the liquid nitrogen charging interface on the top cover C3 of the shot blasting chamber.

[0038] The top cover C3 is also provided with an installation opening for installing a temperature sensor WC.

[0039] The outlet of the one-way throttle valve E3 is connected to the top cover C3 of the shot blasting chamber, and liquid nitrogen is sent into the shot blasting chamber from top to bottom.

[0040] The principle of deep cold strengthening of blade tenon is as follows:

[0041] Since the tenon has an open surface structure, the overall shot peening strengthening method is adopted.

[0042] The ultrasonic generator of the ultrasonic vibration system operates, and the vibration head vibrates at a high frequency, exciting the pellets pre-placed on the top surface of the vibration head to impact the tenon surface at a high frequency, causing the tenon surface material to undergo superstrain plastic deformation, generating dislocations, twins, subgrains, etc., achieving grain refinement, improving the surface hardness of the tenon structure, and implanting high residual compressive stress. At the same time, the cryogenic device injects low-temperature liquid nitrogen into the shot peening chamber, exposing the tenon to a deep-cold environment. This not only prevents oxidation reactions on the workpiece, but also allows nitriding strengthening of the workpiece in the localized temperature increase environment caused by the pellet impact: increasing the plastic flow stress of the metal, which is beneficial for suppressing the dynamic recovery of dislocations and cross-slip, promoting twin nucleation, increasing the probability of martensitic phase transformation, forming nano-fine grains, improving the stability of the reinforced structure, and further increasing the surface hardness and residual compressive stress.

[0043] When the tenon strengthening system and the cryogenic device have been working for a specified time, the motor of the tenon driving device will work to rotate the tenon 180 degrees, and then the tenon strengthening system and the cryogenic device will continue to work for a corresponding time to ensure uniform strengthening of the tenon surface.

[0044] Example 2: This example strengthens the tenon groove surface of the turbine disk of the aviation tenon structure.

[0045] Combine Figure 3-5 As can be seen, the mortise and tenon strengthening system in this embodiment includes a workbench A, a horizontal rotary platform F, a modular slide, an ultrasonic vibration system B, and a pellet circulation device. The mortise and tenon strengthening system is equipped with a cryogenic device E.

[0046] The horizontal rotary platform F for installing the turbine disc WLP is fixed on the workbench A.

[0047] The combined module slide includes a horizontal module slide G and a vertical module slide H connected by its slider. The horizontal module slide is fixed on the side of the workbench corresponding to the horizontal rotary platform F.

[0048] Both the horizontal module slide G and the vertical module slide H use synchronous belt linear module slides.

[0049] The difference between ultrasonic vibration system B and embodiment 1 is:

[0050] The transducer and the amplitude converter are arranged horizontally. The pull rod assembly connected to the amplitude converter is also connected to the slider of the vertical module slide H through the horizontal bracket B6. The vibration head B7 connected to the amplitude converter is inserted into the mortise and tenon, and the vibration head is a contoured structure of the mortise and tenon. After the vibration head is inserted into the mortise and tenon SC, the assembly gap with the mortise and tenon is 2-10mm.

[0051] Since the mortise and tenon of the turbine disc is a three-quarter closed structure and the mortise and tenon is strengthened in a single groove manner, the shot peening strengthening system does not have a shot peening chamber, but a shot circulation device I is provided.

[0052] The pellet circulation device 1 comprises a pellet storage box 11 and a shot blasting pipe 12 and a recovery pipe 13 connected thereto. The end of the shot blasting pipe is connected to a shot blasting gun 14, and the upper end of the recovery pipe is connected to a cone bucket 15. The shot blasting pipe is connected to a pellet delivery pump (not shown). The shot blasting gun is located directly above the vibrating head B7 and blasts the pellets from top to bottom. The cone bucket 15 is fixed to the lower area of ​​the corresponding vibrating head on the workbench, and corresponding cone buckets are provided with corresponding holes on the workbench.

[0053] The difference between the cryogenic device E and the embodiment 1 is that the end of the delivery pipe connected to the liquid nitrogen bottle is connected to the spray gun E4, which is located near the shot blasting gun I4 so that the sprayed liquid nitrogen can cover the shot blasting area.

[0054] The principle of deep cold strengthening of the mortise and tenon in this embodiment is as follows:

[0055] The ultrasonic vibration system's ultrasonic generator operates, causing the vibrating head to vibrate at a high frequency. Simultaneously, a spray gun sprays pellets (1.5 mm in diameter) into the mortise and tenon located at the vibrating head. The pellets impact the mortise and tenon surface at a high frequency within the gap between the vibrating head and the tenon, strengthening it. Because the vibrating head and the tenon and tenon are contoured structures, the uniformity of the mortise and tenon surface strengthening is ensured. Simultaneously, low-temperature liquid nitrogen ejected from the cryogenic device assists in strengthening the surface. The principles of ultrasonic shot peening and liquid nitrogen cryogenic strengthening are the same as those in Example 1 and will not be further elaborated here.

[0056] The worm wheel WLP is in a horizontal state and is rotated by a horizontal rotary platform F.

[0057] After strengthening a mortise, the vibrating head is first withdrawn from the mortise using the horizontal module slide G. The horizontal rotary platform F then operates to rotate the worm gear one mortise position. The vibrating head is then inserted into the new mortise using the horizontal module slide. This mortise is then strengthened until all mortise slots are strengthened. The vertical module slide H adjusts the height of the vibrating head B7 during system assembly.

[0058] Example 3: This example also strengthens the surface of the tenon groove of the turbine disc of the aviation tenon structure.

[0059] Combine Figure 6-7 It can be seen that the difference between the tongue and groove reinforcement system in this embodiment and the second embodiment is:

[0060] The horizontal module slide G and the vertical module slide H are arranged separately, and the vertical rotary platform J for mounting the turbine disc is mounted on the slider of the vertical rotary platform, so that the turbine disc WLP rotates along the vertical plane.

[0061] In this embodiment, the horizontal module slide G and the vertical module slide H respectively adopt a synchronous belt linear module slide and a screw slider linear module slide.

[0062] The vibration head B7 of the ultrasonic vibration system B is vertically inserted into the mortise and tenon, and the support rod assembly connected to the amplitude rod is then connected to the slider of the horizontal module slide G through the bracket B8.

[0063] The shot blasting gun I4 of the shot circulation device I and the liquid nitrogen spray gun E4 of the cryogenic device E correspond to the left and right sides of the vibration head respectively.

[0064] After strengthening one groove, the vertical module slide H is used to raise the turbine disc and separate it from the vibration head, as the height position of the vibration head remains unchanged. The vertical rotary platform J then operates to rotate the turbine disc one groove position. The vertical module slide is then used to return the turbine disc to its original height and cooperate with the vibration head to strengthen the new groove until all grooves are strengthened. The horizontal module slide G is used to adjust the horizontal position of the vibration head during system assembly.

[0065] During the shot peening process of Example 2 and Example 3, the shot pellets after shot peening fall into the cone hopper I5 of the shot circulation device under the action of gravity and then return to the shot storage box to achieve recycling.

Claims

1. A method for strengthening the surface of an aviation tenon structure. Features: The method uses an ultrasonic strengthening system to perform shot peening strengthening on the surface of the tenon structure while using a deep cooling device for auxiliary strengthening; the ultrasonic strengthening system includes a tenon strengthening system and a tenon groove strengthening system, the tenon adopts an overall strengthening method, and the tenon groove adopts a single groove strengthening method; Under the excitation of ultrasonic high-frequency vibration, the pellets impact the surface of the tenon structure at high frequency, promoting super-strain plastic deformation on the surface of the tenon structure, generating dislocations, twins, sub-grains, etc., achieving grain refinement, improving the surface hardness of the tenon structure, and implanting high residual compressive stress; Cryogenic assistance can increase the plastic flow stress of metals, which is beneficial to inhibit the dynamic recovery of dislocations and cross slip, promote twin nucleation, increase the probability of martensitic phase transformation, form nano-fine grains, improve the stability of strengthened structures, and further increase surface hardness and residual compressive stress.

2. The method for strengthening the surface of an aviation tenon structure according to claim 1, Features: The tenon strengthening system includes a workbench, an ultrasonic vibration system, a shot peening chamber and a tenon driving device. The shot peening chamber and the ultrasonic vibration system are both fixed on the workbench. The vibration head connected to the upper end of the amplitude change rod of the ultrasonic vibration system extends into the bottom of the shot peening chamber. The rotating actuator of the tenon driving device extends horizontally into the shot peening chamber above the corresponding vibration head, and the end is connected to a clamp for installing the tenon.

3. The method for strengthening the surface of an aviation tenon structure according to claim 2, Features: The shot peening chamber comprises a cylinder and a base and a top cover connected at both ends thereof, the outer diameter of the base matches the inner diameter of the cylinder, and the top cover is an elliptical cover; the vibration head and the base are clearance-matched, and the clearance is smaller than the diameter of the shot.

4. The method for strengthening the surface of an aviation tenon structure according to claim 2, Features: The tenon drive device comprises a motor, a coupling and the clamp. The motor is arranged with its output shaft in a horizontal direction. The output shaft and the clamp are connected via a coupling to form the rotary actuator.

5. The method for strengthening the surface of an aviation tenon structure according to claim 1, Features: The mortise and tenon strengthening system includes a workbench, a turbine disc drive device, a combined module slide and an ultrasonic vibration system; the turbine disc drive device adopts a horizontal rotating platform, which is fixed on the workbench; the combined module slide includes a horizontal module slide and a vertical module slide connected to its slider, and the horizontal module slide is fixed on the side of the workbench corresponding to the horizontal rotating platform; the transducer and the amplitude rod of the ultrasonic vibration system are arranged horizontally, connected to the slider of the vertical module slide through a horizontal bracket, and the vibration head connected to the amplitude rod is inserted into the mortise and tenon.

6. The method for strengthening the surface of an aviation tenon structure according to claim 1, Features: The mortise and tenon strengthening system comprises a workbench, a turbine disc driving device, a vertical module slide, a horizontal module slide and an ultrasonic vibration system; the vertical module slide is fixed on the workbench, the turbine disc driving device adopts a vertical rotary table, and the vertical rotary platform is connected to the slider of the vertical module slide; the horizontal module slide is fixed on the workbench, the transducer and the amplitude rod of the ultrasonic vibration system are arranged vertically, connected to the slider of the horizontal module slide through a combined bracket, and the vibration head connected to the amplitude rod is inserted into the mortise and tenon.

7. The method for strengthening the surface of an aviation tenon structure according to claim 6, Features: An auxiliary bracket is arranged on the rear side of the workbench corresponding to the vertical module slide, and a clamping plate for connecting the auxiliary bracket is arranged on the rear side of the vertical module slide.

8. The method for strengthening the surface of an aviation tenon structure according to claim 5 or 6, Features: The mortise and tenon strengthening system also includes a shot circulation device, which includes a shot storage box and a shot peening pipe and a recovery pipe connected thereto. The shot peening pipe is connected to a shot conveying pump, the end of the shot peening pipe is connected to a shot peening gun, and the end of the recovery pipe is connected to a cone bucket. The shot peening gun is located directly above the vibration head, and the cone bucket is fixed on the workbench in the area below the corresponding vibration head, and a corresponding hole is opened on the workbench at the corresponding cone bucket.

9. The method for strengthening the surface of an aviation tenon structure according to claim 5 or 6, Features: The shape of the vibration head matches the mortise and tenon, and the assembly gap is 2-10mm.

10. The method for strengthening the surface of an aviation tenon structure according to claim 1, Features: The cryogenic device comprises a liquid nitrogen bottle and a nitrogen delivery pipeline connected thereto.

Citation Information

Cited By

  • Ultrasonic vibration auxiliary processing parameter mapping method for cross-scale bridging index

    CN121340041A