Hyperbranched triazine carbonizing agent, composite flame retardant and flame retardant polypropylene material
Through the combination of hyperbranched triazine carbonization agent with piperazine pyrophosphate composite and modified nickel-aluminum hydrotalcite-montmorillonite nanocomposite, the problem of poor water resistance of expanded flame retardants in polypropylene materials is solved, and the problem of poor water resistance of expanded flame retardants in polypropylene materials is improved. Flame retardant smoke suppression and mechanical properties meet environmental protection needs and are close to the performance of pure PP.
Patent Information
- Application Number
- CN202411314880.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-20
AI Technical Summary
Traditional expansion flame retardants have poor water resistance and easy migration, which leads to their unsatisfactory flame retardant effects in polypropylene materials, and halogen-containing flame retardants produce toxic gases during incineration, affecting environmental protection needs.
Hyperbranched triazine carbonization agent is used to combine with piperazine pyrophosphate, and combined with modified nickel-aluminum hydrotalcite-montmorillonite nanocomposites to form a composite expanded flame retardant, improving the water resistance and flame retardant and smoke inhibition of polypropylene materials Performance, and porous structures are formed by urea hydrothermal method and alkali corrosion treatment to improve mechanical properties.
It has achieved the improvement of the flame retardant and mechanical properties of polypropylene materials, good water resistance, and no toxic gases to produce, meet environmental protection needs, and is close to or even exceeds the mechanical properties of pure PP.
Smart Images

Figure CN118812848B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardants, and in particular to a hyperbranched triazine carbonizing agent, a composite flame retardant and a flame retardant polypropylene material. Background Art
[0002] Polypropylene (PP) is a thermoplastic made from propylene monomers. It is lightweight, strong, chemically resistant, electrically insulating, and has excellent formability, making it widely used in packaging, automobiles, home appliances, building materials, textiles, and other fields. Polypropylene is flammable and releases toxic gases and smoke when burned, which leads to many problems in daily applications, such as fire safety and environmental hazards. Adding flame retardants is an economical and efficient solution to improve the fire safety of polypropylene materials.
[0003] Flame retardants are functional additives added to plastics, wood or textiles to reduce their flammability. They are used to inhibit, suppress or delay the generation of flames and prevent the spread of fire. Traditional halogen-containing flame retardants usually produce small amounts of dioxins or dibenzofurans when heated, and plastics containing these flame retardants are not suitable for recycling or incineration. Therefore, with the increasing demand for environmental protection, it has become crucial to develop new, environmentally friendly and efficient flame retardants.
[0004] Intumescent flame retardant (IFR) is a new type of green flame retardant with the characteristics of high safety, halogen-free, low smoke generation, low toxicity, and no corrosive gas generation. The main components of the intumescent flame retardant system include acid source (dehydrating agent), carbon source (carbon-forming agent) and gas source (foaming agent). These three components work synergistically during the combustion process to exert excellent flame retardant effect. The most commonly used intumescent flame retardant is a compound system with ammonium polyphosphate (APP) as the acid source. However, APP is easy to absorb moisture and migrate. Intumescent flame retardants based on APP generally have disadvantages such as poor water resistance and easy migration, which reduces the flame retardant effect. Piperazine pyrophosphate (PAPP) is a new type of intumescent flame retardant with better flame retardancy, heat resistance and water resistance, but its flame retardant effect is not ideal when used alone. In order to achieve higher fire safety, it is necessary to find a PAPP compound intumescent flame retardant system with excellent water resistance and flame retardant and smoke suppression effects. Summary of the invention
[0005] Based on the technical problems existing in the background technology, the present invention proposes a hyperbranched triazine carbonizing agent, a composite flame retardant and a flame retardant polypropylene material.
[0006] The present invention provides a hyperbranched triazine carbon-forming agent, the structural formula of which is shown in Formula I:
[0007]
[0008] Formula Ⅰ.
[0009] The hyperbranched triazine carbon former represented by formula I is hereinafter referred to as carbon former PCAT.
[0010] Preferably, the hyperbranched triazine carbon-forming agent is prepared by polycondensation reaction in a solvent using cyanuric chloride and 3-amino-1,2,4-triazole as monomers in the presence of an acid-binding agent.
[0011] Preferably, the acid binding agent is NaOH.
[0012] Preferably, the molar ratio of cyanuric chloride to 3-amino-1,2,4-triazole is 1:1.5-2.
[0013] Preferably, the preparation method of the hyperbranched triazine carbon-forming agent comprises the following steps:
[0014] (1) Dissolve 0.1 mol of cyanuric chloride in 1,4-dioxane to obtain a cyanuric chloride solution; dissolve 0.15-0.2 mol of 3-amino-1,2,4-triazole in water to obtain a 3-amino-1,2,4-triazole solution; mix the 3-amino-1,2,4-triazole solution with the cyanuric chloride solution, dropwise add an aqueous solution of an inorganic base, control the pH to 8-9, and react at -5-5°C for 2-3 hours;
[0015] (2) adding an aqueous solution of an inorganic base to the material obtained in step (1), controlling the pH to 8-9, and reacting at 45-55°C for 2-3 hours;
[0016] (3) Add an aqueous solution of an inorganic base to the material obtained in step (2), control the pH to 8-9, react at 85-95° C. for 6-8 hours, and after the reaction is completed, filter, wash, and dry to obtain the product; the inorganic base is sodium hydroxide, potassium hydroxide, or a combination thereof.
[0017] Preferably, in step (1), the molar ratio of the inorganic base to cyanuric chloride is 1-1.5:1; in step (2), the molar ratio of the inorganic base to cyanuric chloride in step (1) is 1-1.5:1; in step (3), the molar ratio of the inorganic base to cyanuric chloride in step (1) is 1-1.5:1.
[0018] The synthetic route of carbon forming agent PCAT is as follows: Figure 1 shown.
[0019] A composite flame retardant, the components of which include piperazine pyrophosphate and the hyperbranched triazine carbon-forming agent; in the composite flame retardant, the mass ratio of piperazine pyrophosphate to the hyperbranched triazine carbon-forming agent is 2:1-3:1.
[0020] Preferably, the components of the composite flame retardant are composed of piperazine pyrophosphate, the hyperbranched triazine carbon-forming agent and a modified nickel aluminum hydrotalcite-montmorillonite nanocomposite material; the mass ratio of the piperazine pyrophosphate to the hyperbranched triazine carbon-forming agent is 2:1-3:1, and the sum of the masses of piperazine pyrophosphate and the hyperbranched triazine carbon-forming agent accounts for 80-85% of the total mass of the composite flame retardant; the mass of the modified nickel aluminum hydrotalcite-montmorillonite nanocomposite material accounts for 15-20% of the total mass of the composite flame retardant;
[0021] The preparation method of the modified nickel-aluminum hydrotalcite-montmorillonite nanocomposite material comprises the following steps:
[0022] (a) dissolving 0.01 mol aluminum nitrate nonahydrate and 0.03 mol nickel nitrate hexahydrate in water to obtain a precursor solution; adding montmorillonite to the precursor solution and uniformly dispersing it by ultrasonication, then adding 0.13-0.14 mol urea and mixing them uniformly, and performing a hydrothermal reaction; after the reaction is completed, centrifuging, washing, and drying to obtain a nickel-aluminum hydrotalcite-montmorillonite composite; wherein the ratio of the mass of the montmorillonite to the sum of the mass of the aluminum nitrate nonahydrate and the mass of the nickel nitrate hexahydrate is 0.5-1:1;
[0023] (b) adding the nickel aluminum hydrotalcite-montmorillonite composite to an aqueous solution of an inorganic base with a concentration of 5-6 mol / L, dispersing the composite uniformly, etching, and then centrifuging, washing and drying the obtained precipitate to obtain the modified nickel aluminum hydrotalcite-montmorillonite nanocomposite material; the inorganic base is sodium hydroxide, potassium hydroxide or a combination thereof.
[0024] Preferably, in step (a), the temperature of the hydrothermal reaction is 100-140° C., and the time is 10-18 hours.
[0025] Preferably, in step (b), the etching temperature is 25-40° C. and the etching time is 12-18 hours.
[0026] A flame retardant polypropylene material comprises PP and a flame retardant, wherein the flame retardant is the composite flame retardant, and the mass of the flame retardant accounts for 18-20% of the total mass of the flame retardant polypropylene material.
[0027] The beneficial effects of the present invention are as follows:
[0028] The present invention compounds a hyperbranched triazine charring agent (PCAT charring agent) containing both a triazine group and a triazole group as shown in Formula I with piperazine pyrophosphate in a suitable ratio to obtain a composite intumescent flame retardant with excellent flame retardant properties. The composite intumescent flame retardant is applied to the flame retardancy of polypropylene materials, so that the polypropylene composite material has both excellent water resistance and high-efficiency flame retardant and smoke suppression properties.
[0029] Furthermore, the present invention can play a synergistic role by introducing an appropriate amount of modified nickel-aluminum hydrotalcite-montmorillonite nanocomposite material into the above-mentioned flame retardant compound system, so that the obtained composite flame retardant can achieve mechanical properties close to or even exceeding those of pure PP while ensuring excellent water resistance and flame retardant and smoke suppression effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is the synthetic route of the carbon-forming agent PCAT.
[0031] Figure 2 FT-IR spectra of carbon-forming agents PCAT, 3-amino-1,2,4-triazole (ATA) and cyanuric chloride (CYC).
[0032] Figure 3 The carbon-forming agent PCAT synthesized by the present invention 13 C solid state NMR spectrum.
[0033] Figure 4 TG and DTG curves of the carbon-forming agent PCAT synthesized in the present invention. DETAILED DESCRIPTION
[0034] The technical solution of the present invention is described in detail below through specific embodiments. Example 1
[0035] The hyperbranched triazine carbon-forming agent (carbon-forming agent PCAT) shown in the synthetic formula I is:
[0036]
[0037] Formula I
[0038] (1) Dissolve 0.1 mol of cyanuric chloride in 120 mL of 1,4-dioxane to obtain a cyanuric chloride solution; dissolve 0.153 mol of 3-amino-1,2,4-triazole in 100 mL of water to obtain a 3-amino-1,2,4-triazole solution; mix the 3-amino-1,2,4-triazole solution with the cyanuric chloride solution, dropwise add an aqueous solution of NaOH (containing 0.1 mol of NaOH), control the pH to 8-9, and react at -5-5°C for 2 h;
[0039] (2) adding an aqueous solution of NaOH (containing 0.1 mol NaOH) dropwise to the material obtained in step (1), controlling the pH to 8-9, and reacting at 45-55°C for 2 h;
[0040] (3) Add an aqueous solution of NaOH (containing 0.1 mol NaOH) dropwise to the material obtained in step (2), control the pH to 8-9, and react at 85-95°C for 6 h. After the reaction is completed, filter, wash, and dry to obtain a product.
[0041] The product samples were scanned using a Nicolet MAGNA-IR 750 FT-IR spectrometer. The chemical structure of the product was characterized by analyzing its Fourier transform infrared spectrum. The infrared spectrum scanning range was 4000~400cm -1 , infrared samples were prepared using potassium bromide tablets. Figure 2 The FT-IR spectra of the carbon-forming agents PCAT, 3-amino-1,2,4-triazole (ATA) and cyanuric chloride (CYC) are shown. Figure 2 From top to bottom, the carbon-forming agents are PCAT, ATA and CYC. In the infrared spectrum, at 3319 cm -1 There is a broad absorption peak near 1645cm, which belongs to the NH vibration absorption peak. -1 and 1211cm -1 The absorption peaks at 1542 cm -1 The broad and strong absorption peaks at 804 cm -1 The sharp absorption peaks at 1290 cm-1 are the characteristic absorption peaks of the triazine ring. This confirms the presence of triazine and triazole groups in the structure of the synthesized compound. -1 A new absorption peak appears at 850 cm-1, which corresponds to the stretching vibration of the CN bond produced by the reaction, indicating that the Cl atom on the triazine ring reacts with 3-amino-1,2,4-triazole. In addition, there is no C-Cl (850 cm-1) in the PCAT spectrum. -1 ), which means that all the chlorine atoms on cyanuric chloride are completely replaced. The existence and disappearance of these characteristic absorption peaks preliminarily prove the successful synthesis of the carbon-forming agent PCAT.
[0042] The product samples were scanned using a Bruker AVANCE III 400WB NMR spectrometer. 13 C absorption peak. 13 The molecular structure of the product was characterized by C solid-state nuclear magnetic resonance spectroscopy at a magnetic field of 400 MHz. Figure 3 PCAT is a carbon forming agent. 13 C solid-state NMR spectrum. The peak at 149.98 ppm corresponds to the tertiary carbon atom in the triazole ring (b), the peak at 57.42 ppm is attributed to the quaternary carbon atom in the triazole ring (c), and the signal at 161.33 ppm belongs to the carbon atom on the triazine ring (a). These results indicate that the product contains triazine and triazole ring structural units, further confirming the condensation reaction of cyanuric chloride and 3-amino-1,2,4-triazole.
[0043] The content of C, H and N in the product was determined by Vario EL CHNS / O element analyzer. The data are shown in Table 1:
[0044] Table 1
[0045]
[0046] It can be seen from Table 1 that the C, H and N contents of the carbon-forming agent PCAT measured and calculated theoretically are almost the same, which are 36.35wt%, 2.21wt% and 61.44wt% and 35.97wt%, 1.50wt% and 62.53%, respectively. By comparing the actual and theoretical values of the elements contained in the carbon-forming agent PCAT, it is proved that the structure of the synthesized carbon-forming agent PCAT is in line with expectations.
[0047] The product samples were tested using a German STA449F3 thermal analyzer, and the thermal stability of the product was analyzed using the thermogravimetric curve obtained. The test temperature range was 35~800℃, the heating rate was 10℃ / min, and it was carried out under a nitrogen atmosphere. Figure 4 The TG and DTG curves of the carbonizing agent PCAT. Calculated at 5% mass loss, the initial decomposition temperature of PCAT is 230℃, which can meet the processing requirements of PP. PCAT decomposes in two steps: the first step ends at 230℃~550℃, with a mass loss of 37.4% and a residual amount of 57.5%, which is mainly due to the breakage of the chemical bonds of its macromolecular main chain. The second step of decomposition occurs at 550℃~750℃, and the mass loss of this part of the decomposition reaches 49.6%. The highest peak temperature of degradation is 690℃, and the final non-combustible residue mass remains 8.1%. At this stage, under high temperature environment, PCAT and its cracking products will undergo strong thermal degradation, and only a small part of the skeleton structure will form non-combustible residues. The complex physical and chemical behavior leads to the opening of triazole rings and triazine rings, and further cross-linking. At the same time, a large amount of non-combustible gas will be generated by a large amount of thermal degradation. At 600℃, PCAT retains about 53.6% of the residue, which is a fairly high residual percentage. If the second stage decomposition of PCAT can be suppressed in the intumescent flame retardant system, an excellent carbonization effect can be achieved. From the above description, it can be seen that the residual carbon of PCAT at 600°C before secondary decomposition can reach 53.6%, which makes it have the potential to be used as an efficient carbonization aid. The high proportion of nitrogen in its molecular structure can also allow it to produce sufficient non-flammable phase components, and it has the potential to be used as a foaming aid. Therefore, PCAT exhibits excellent carbonization performance under appropriate conditions, and its high nitrogen content has the potential to produce excellent foaming performance. Example 2
[0048] Prepare single component flame retardant or composite flame retardant according to the raw material formula in Table 2:
[0049] Table 2
[0050]
[0051] In Table 2:
[0052] The inorganic filler A is montmorillonite.
[0053] The inorganic filler B is nickel-aluminum hydrotalcite, and its preparation method is as follows:
[0054] Dissolve 0.01 mol aluminum nitrate nonahydrate and 0.03 mol nickel nitrate hexahydrate in 500 mL water to obtain a precursor solution; add 0.132 mol urea to the precursor solution and mix well, and perform hydrothermal reaction at 140° C. for 12 hours. After the reaction is completed, centrifuge, wash, and dry to obtain nickel-aluminum hydrotalcite.
[0055] The inorganic filler C is a nickel-aluminum hydrotalcite-montmorillonite nanocomposite material, and its preparation method is as follows:
[0056] 0.01 mol aluminum nitrate nonahydrate and 0.03 mol nickel nitrate hexahydrate were dissolved in 500 mL water to obtain a precursor solution; 8.5 g montmorillonite was added to the precursor solution and dispersed evenly by ultrasonic, and then 0.132 mol urea was added and mixed evenly, and a hydrothermal reaction was carried out at 140° C. for 12 hours. After the reaction was completed, the mixture was centrifuged, washed, and dried to obtain a nickel-aluminum hydrotalcite-montmorillonite composite material.
[0057] The inorganic filler D is a modified nickel-aluminum hydrotalcite-montmorillonite nanocomposite material, and its preparation method is as follows:
[0058] (a) 0.01 mol aluminum nitrate nonahydrate and 0.03 mol nickel nitrate hexahydrate were dissolved in 500 mL water to obtain a precursor solution; 8.5 g montmorillonite was added to the precursor solution and dispersed uniformly by ultrasonication, and then 0.132 mol urea was added and mixed uniformly, and the mixture was hydrothermally reacted at 140° C. for 12 h. After the reaction was completed, the mixture was centrifuged, washed, and dried to obtain a nickel-aluminum hydrotalcite-montmorillonite composite;
[0059] (b) The nickel-aluminum hydrotalcite-montmorillonite composite was evenly dispersed in 100 mL of a 5 mol / L NaOH aqueous solution, etched at 35° C. for 15 h, and then centrifuged. The obtained precipitate was washed and dried to obtain a modified nickel-aluminum hydrotalcite-montmorillonite nanocomposite material.
[0060] The flame retardant in Table 2 was used to prepare polypropylene material samples, and the formula is shown in Table 3. All raw materials were dried overnight in a vacuum oven at 80°C before preparation. The preparation method is as follows: first add PP to a mixer, and after it is completely melted, add the remaining raw materials, and mix for 25 minutes at 180°C and a roller speed of 35rpm, then cut into pellets, and place the pellets in a mold, and hot press at 180°C and 8MPa for 5 minutes to obtain a test sample of the polypropylene material. The performance of the prepared polypropylene material sample was tested, and the test method is as follows:
[0061] 1. Flame retardant performance test
[0062] (1) Limiting oxygen index (LOI)
[0063] According to ASTM D2863-97, LOI was measured using a JF-3 oxygen index instrument from Jiangning Analytical Instrument Co., Ltd., China, and the size of the measured sample was 100 mm × 6.5 mm × 3 mm.
[0064] (2) Vertical burning test (UL-94)
[0065] According to ASTMD3801 standard, UL-94 test was carried out using PX-03-001 vertical combustion apparatus produced by China Phoenix Quality Inspection Instrument Co., Ltd. The size of the test sample was 150 mm × 75 mm × 3 mm.
[0066] 2. Mechanical properties test
[0067] The tensile strength and elongation at break were measured according to GB / T1040.2-2006 using an electronic universal mechanical testing machine (E44.104, China Wanshida Co., Ltd.). The specimens were cut into a size of 75 mm × 5 mm × 2 mm.
[0068] The above performance test results are shown in Table 3.
[0069] Table 3
[0070]
[0071] According to the comparison of the test data of samples PP-0~7 in Table 3, it can be seen that the present invention can obtain a composite intumescent flame retardant with excellent flame retardant properties by compounding the hyperbranched triazine charring agent containing both triazine groups and triazole groups with piperazine pyrophosphate at a suitable ratio. The composite intumescent flame retardant is applied to the flame retardant of polypropylene materials, so that the polypropylene composite material has high efficient flame retardant and smoke suppression properties.
[0072] According to the comparison of the test data of PP-0, PP-3 and PP-8~14 in Table 3, it can be seen that the introduction of an appropriate amount of modified nickel-aluminum hydrotalcite-montmorillonite nanocomposite material into the flame retardant can further achieve mechanical properties close to or even exceeding those of pure PP while ensuring excellent flame retardant and smoke suppression effects. This is because the present invention obtains a composite of montmorillonite and hydrotalcite by a urea hydrothermal method, and then obtains a modified nickel aluminum hydrotalcite-montmorillonite nanocomposite material with porous characteristics by alkaline corrosion treatment, and cooperates with an intumescent flame retardant to obtain a composite flame retardant. This modified nickel aluminum hydrotalcite-montmorillonite nanocomposite material has a uniform three-dimensional structure and a large number of functional groups. It can effectively improve the mechanical properties of the material by constructing a three-dimensional network structure in the polypropylene material and interacting with the functional groups on the hyperbranched triazine carbonizing agent; the loading of nickel aluminum hydrotalcite on the surface of montmorillonite can play a catalytic role in promoting carbonization and good smoke suppression performance, and the rich porous structure formed by alkaline corrosion can alleviate the barrier effect of the montmorillonite and hydrotalcite layered structure on the non-combustible gas generated by the flame retardant during combustion when the dosage is large, thereby avoiding the barrier of the non-combustible gas and the inability to form a carbon layer with a good expansion degree, so that the mechanical properties of the polypropylene composite material can reach a level close to or even exceed that of pure PP, while ensuring an excellent flame retardant effect.
[0073] 3. Water resistance test
[0074] After the sample was immersed in 80°C distilled water for 168 hours, it was dried in a vacuum drying oven. The water resistance of the material was evaluated by the change of UL-94 grade. The test results showed that the UL-94 grade of polypropylene material samples PP-3, 4, 12, and 13 after being immersed in water for 168 hours could all be maintained at V-0 grade, indicating that the composite flame retardant of the present invention has excellent water resistance.
[0075] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A composite flame retardant, characterized in that: The components of the composite flame retardant are composed of piperazine pyrophosphate, a hyperbranched triazine carbon former and a modified nickel aluminum hydrotalcite-montmorillonite nanocomposite material; the mass ratio of the piperazine pyrophosphate to the hyperbranched triazine carbon former is 2:1-3:1, the sum of the mass of the piperazine pyrophosphate and the hyperbranched triazine carbon former accounts for 80-85% of the total mass of the composite flame retardant; the mass of the modified nickel aluminum hydrotalcite-montmorillonite nanocomposite material accounts for 15-20% of the total mass of the composite flame retardant; The structural formula of the hyperbranched triazine carbon-forming agent is shown in Formula I: ; Formula I The preparation method of the modified nickel-aluminum hydrotalcite-montmorillonite nanocomposite material comprises the following steps: (a) dissolving 0.01 mol aluminum nitrate nonahydrate and 0.03 mol nickel nitrate hexahydrate in water to obtain a precursor solution; adding montmorillonite to the precursor solution and uniformly dispersing it by ultrasonication, then adding 0.13-0.14 mol urea and mixing them uniformly, and performing a hydrothermal reaction; after the reaction is completed, centrifuging, washing, and drying to obtain a nickel-aluminum hydrotalcite-montmorillonite composite; wherein the ratio of the mass of the montmorillonite to the sum of the mass of the aluminum nitrate nonahydrate and the mass of the nickel nitrate hexahydrate is 0.5-1:1; (b) adding the nickel aluminum hydrotalcite-montmorillonite composite to an aqueous solution of an inorganic base with a concentration of 5-6 mol / L, dispersing the composite uniformly, etching, and then centrifuging, washing and drying the obtained precipitate to obtain the modified nickel aluminum hydrotalcite-montmorillonite nanocomposite material; the inorganic base is sodium hydroxide, potassium hydroxide or a combination thereof.
2. The composite flame retardant according to claim 1, characterized in that: The hyperbranched triazine carbonizing agent is prepared by polycondensation reaction in a solvent with cyanuric chloride and 3-amino-1,2,4-triazole as monomers in the presence of an acid-binding agent.
3. The composite flame retardant according to claim 2, characterized in that: The molar ratio of cyanuric chloride to 3-amino-1,2,4-triazole is 1:1.5-2.
4. The composite flame retardant according to claim 1, characterized in that: The preparation method of the hyperbranched triazine carbon-forming agent comprises the following steps: (1) Dissolve 0.1 mol of cyanuric chloride in 1,4-dioxane to obtain a cyanuric chloride solution; dissolve 0.15-0.2 mol of 3-amino-1,2,4-triazole in water to obtain a 3-amino-1,2,4-triazole solution; mix the 3-amino-1,2,4-triazole solution with the cyanuric chloride solution, dropwise add an aqueous solution of an inorganic base, control the pH to 8-9, and react at -5-5°C for 2-3 hours; (2) adding an aqueous solution of an inorganic base to the material obtained in step (1), controlling the pH to 8-9, and reacting at 45-55°C for 2-3 hours; (3) Add an aqueous solution of an inorganic base to the material obtained in step (2), control the pH to 8-9, react at 85-95° C. for 6-8 hours, and after the reaction is completed, filter, wash, and dry to obtain the product; the inorganic base is sodium hydroxide, potassium hydroxide, or a combination thereof.
5. The composite flame retardant according to claim 4, characterized in that: In step (1), the molar ratio of the inorganic base to cyanuric chloride is 1-1.5:1; in step (2), the molar ratio of the inorganic base to cyanuric chloride in step (1) is 1-1.5:1; in step (3), the molar ratio of the inorganic base to cyanuric chloride in step (1) is 1-1.5:
1.
6. The composite flame retardant according to claim 1, characterized in that: In step (a), the temperature of the hydrothermal reaction is 100-140° C. and the time is 10-18 hours.
7. The composite flame retardant according to claim 1, characterized in that: In step (b), the etching temperature is 25-40° C. and the etching time is 12-18 hours.
8. A flame retardant polypropylene material, characterized in that: The invention comprises PP and a flame retardant, wherein the flame retardant is the composite flame retardant according to any one of claims 1 to 7, and the mass of the flame retardant accounts for 18 to 20% of the total mass of the flame retardant polypropylene material.
Citation Information
Cited By
A halogen-free flame-retardant long-glass-fiber-reinforced polypropylene composite material and a preparation method thereof
CN122978592A