Lithium ion battery silicon negative electrode binder and preparation method and application thereof

By using a three-dimensional binder with both covalent cross-linking network and dynamic supramolecular interaction in lithium-ion batteries, the problem of electrode structure damage caused by volume changes of the silicon anode is solved, and the electrochemical performance and cycle stability are significantly improved, achieving High-capacity and long-life lithium-ion battery anode.

CN118813166AActive Publication Date: 2024-10-22ZHEJIANG UNIV +1

Patent Information

Application Number
CN202410828495.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-22
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

Existing lithium-ion battery silicon anode materials undergo large volume changes during the lithiation/delithiation process, resulting in electrode structure damage and electrochemical performance deterioration. Traditional binders cannot effectively limit volume expansion, resulting in limited discharge capacity and cycle performance.

Method used

Using a three-dimensional binder with both covalent cross-linking network and dynamic supramolecular effects, the monomer of the phenol group is grafted through the amidation reaction or esterification reaction, and a cross-linking agent is added to form a strong covalent ester bond and a dynamic supramolecular bond. The molecular action sites build a stable three-dimensional network to improve the mechanical properties of the binder and the structural integrity of the electrode.

Benefits of technology

Effectively suppresses the volume deformation of the silicon anode during cycling and improves electrochemical performance. The nano-silicon anode exhibits high discharge capacity, good rate performance and long cycle life, and can still retain its performance after 500 cycles at a current density of 2A/g. It has a high capacity of 1738mAh/g and a cycle life of up to 800 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118813166A_ABST
    Figure CN118813166A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium ion battery silicon negative electrode binder with a chemical and physical double cross-linked network as well as a preparation method and application of the lithium ion battery silicon negative electrode binder. The binder is prepared by grafting a monomer containing a phenol group through an amidation reaction of a high-molecular polymer and then adding a cross-linking agent for a thermal cross-linking reaction. The flexible polysaccharide is modified by phenol, so that the adhesive is endowed with abundant hydrogen bonds and relatively strong viscoelasticity, and stress generated by volume expansion of silicon is effectively dissipated through reversible dissociation-recombination based on dynamic bonds of hydroxyl, carboxyl and acylamino. In addition, carboxyl of the cross-linking agent and hydroxyl of polysaccharide are subjected to in-situ thermal cross-linking to form strong covalent ester bonds, so that the mechanical property of the silicon negative electrode is improved, and the cycling stability of the silicon negative electrode is improved. The silicon negative electrode containing the binder disclosed by the invention can still retain the high capacity of 1738mAh / g after being circulated for 500 circles under the current density of 2A / g, and the cycle life is as long as 800 circles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium ion batteries, and in particular to a silicon negative electrode binder for lithium ion batteries and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have become one of the most widely studied energy storage systems due to their high energy density, high output voltage, long cycle life and environmental friendliness. However, common graphite-based carbon-based negative electrode materials are close to their theoretical specific capacity (372mAh / g). In order to meet the growing energy density requirements of portable electronic devices and electric vehicles, a large amount of research is devoted to promoting the development of high-capacity electrodes for lithium-ion batteries. Silicon has a higher theoretical capacity (4200mAh g -1 ) and low operating voltage (0.4V), making it one of the candidates for high-capacity anodes. However, there is a huge volume change (300%) when silicon is deintercalated with lithium, which can cause problems such as electrode structure destruction and instability of the solid electrolyte interface film, leading to deterioration of electrochemical performance. Commonly used strategies such as nanostructure design, composite with other materials, and pre-lithiation are used to solve the problems of silicon anodes, but these strategies often involve complex preparation processes and high costs. In contrast, binder design shows good prospects in improving the electrochemical stability of silicon anodes due to its versatility and economic practicality.

[0003] Traditional PVDF binders cannot withstand the volume changes of silicon materials due to weak intermolecular van der Waals forces. In recent years, biomass materials have become a research hotspot for silicon negative electrode binders due to their rich polar functional groups and unique structures that produce strong and reversible dynamic secondary bonds. However, the physical cross-linking network of the binder alone is still not enough to fully limit the severe volume expansion effect of silicon. Its molecular chains can easily detach from the surface of silicon particles and even suffer structural damage. The silicon negative electrode only exhibits limited discharge capacity and cycle performance. Therefore, in order to improve the electrochemical performance of silicon negative electrodes, higher requirements are placed on the design and preparation of binders. Summary of the invention

[0004] The present invention aims at the deficiencies of the prior art and provides a silicon negative electrode binder having both a covalent cross-linked network and a dynamic supramolecular effect, so as to solve the problem that the existing linear polymer binder is prone to bonding failure when subjected to stress, effectively inhibit the volume deformation of the silicon negative electrode during the cycle process and improve its electrochemical performance. At the same time, the present invention also provides a preparation method of the binder and its application in lithium-ion batteries.

[0005] In order to achieve the above-mentioned object of the invention, the present invention is implemented through the following technical solutions.

[0006] The present invention first provides a lithium ion battery silicon negative electrode binder, which is a cross-linked three-dimensional network binder, that is, a binder containing a double cross-linked network of chemical cross-linking and physical cross-linking; the chemical cross-linking refers to a cross-linked network containing covalent ester bonds, and the physical cross-linking refers to a cross-linked network containing dynamic supramolecular action sites.

[0007] The present invention also provides a method for preparing the above-mentioned silicon negative electrode binder for lithium ion batteries, the preparation method being: after dissolving a high molecular polymer in a solvent, grafting a monomer containing a phenol group through an amidation reaction or an esterification reaction, and then adding a crosslinking agent for a thermal crosslinking reaction. The high molecular polymer is grafted with a monomer containing a phenol group through an amidation reaction or an esterification reaction to increase the hydrogen bonding sites between the binder and the silicon particles; then a crosslinking agent is added to perform thermal crosslinking to form a strong covalent ester bond, thereby improving its mechanical properties and ensuring the integrity of the electrode structure. A three-dimensional network binder having both dynamic supramolecular action and ester bond covalent action is formed through two-step modification. The covalent bonds in the crosslinked network have the characteristics of high dissociation energy and not easy to break, so the mechanical properties of the binder of the present invention can be improved through covalent chemical crosslinking, and a more stable bonding network can be constructed to three-dimensionally fix silicon particles and withstand most of the stress generated during the silicon lithiation / delithiation process. At the same time, the dynamic supramolecular action is combined to dissipate the residual stress and prevent the polymer molecular chain from structural damage, thereby improving the cycle life of the silicon negative electrode.

[0008] The high molecular polymer includes one or more of hyaluronic acid, sodium alginate, sodium carboxymethyl cellulose, xanthan gum, peach gum, gellan gum and gum arabic.

[0009] The monomer containing a phenol group includes at least one of dopamine, 5-hydroxydopamine, gallic acid, tannic acid and derivatives thereof.

[0010] The cross-linking agent is at least one of iminodiacetic acid, oxalic acid, malonic acid, tartronic acid, succinic acid, adipic acid, suberic acid, and 1,3-acetone dicarboxylic acid.

[0011] The usage amounts of the monomer containing phenol groups and the high molecular polymer satisfy that the phenol groups account for 5% to 15% of the total amount of carboxyl groups in the high molecular polymer.

[0012] The mass ratio of the high molecular weight polymer to the cross-linking agent is 4:1 to 1:1.

[0013] Furthermore, the molecular weight of the high molecular weight polymer is ≥ 100,000, preferably about 400,000. For example, the hyaluronic acid used in the embodiments of the present invention has a molecular weight of 200,000, 400,000, or 600,000.

[0014] More specifically, the preparation method of the above-mentioned lithium-ion battery silicon negative electrode binder includes the following specific steps.

[0015] S1. Dissolve the polymer in a solvent, add an amidation reagent and stir thoroughly, then add a monomer containing a phenol group and react for 6 to 48 hours under argon or nitrogen. The reaction process is carried out in the dark and in an anaerobic environment, and the grafted product is obtained by dialysis and freeze-drying.

[0016] S2. The grafted product and the cross-linking agent are mixed in a certain mass ratio and dissolved in deionized water to prepare a binder precursor solution.

[0017] S3. The binder precursor solution is subjected to heat treatment in a vacuum oven at 120 to 180° C. for 1 to 12 hours to undergo a thermal crosslinking reaction to obtain the binder.

[0018] The solvent in step S1 is at least one of deionized water, phosphate buffer, and 4-morpholineethanesulfonic acid buffer with a pH value of ≤7.

[0019] The amidation agent is at least one of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and derivatives thereof.

[0020] The dialysis in step S1 is performed using deionized water with a pH value of ≤7 for 2 to 5 days.

[0021] The present invention also provides a method for preparing a negative electrode of a lithium ion battery, comprising the following steps:

[0022] The negative electrode active material, the conductive additive and the binder precursor solution mentioned above are weighed in a certain mass ratio, and the three are mixed to form a uniform negative electrode slurry.

[0023] The mass ratio of the negative electrode active material, the conductive additive and the binder precursor solution is 60-80:10-20:10-20.

[0024] According to 0.5~1.0mg / cm 2 The negative electrode slurry is coated on a copper foil, dried in a vacuum drying oven at 60-80°C for 8-12 hours to obtain a pole piece with a complete surface, and then the pole piece is placed in a vacuum drying oven at 120-180°C for 1-12 hours for heat treatment to obtain the negative electrode of the lithium ion battery. During the heat treatment process, the carboxyl group of the cross-linking agent in the binder precursor solution and the hydroxyl group of the polymer polysaccharide are in-situ thermally cross-linked to form a strong covalent ester bond.

[0025] In the present invention, the negative electrode active material is at least one of nano-silicon, micro-silicon, and silicon-carbon material.

[0026] The conductive additive is at least one of Super P, conductive carbon black, conductive graphite, acetylene black, Ketjen black, carbon nanotubes and carbon fibers.

[0027] The beneficial effects of the present invention are:

[0028] The binder of the present invention adopts a phenol group with strong wet adhesion to modify a flexible high molecular polymer, which gives the binder abundant hydrogen bonds and strong viscoelasticity. The dynamic bonds based on hydroxyl, carboxyl and amide groups, i.e., dynamic supramolecular, effectively dissipate the stress generated by the volume expansion of silicon through reversible dissociation-recombination. In addition, the carboxyl group of the crosslinking agent and the hydroxyl group of the high molecular polysaccharide are in situ thermally crosslinked to form a strong covalent ester bond to improve its mechanical properties. A two-step modification is adopted to obtain a bonding network with both dynamic supramolecular action and ester bond covalent action. The binder is given a high Young's modulus, damage resistance and strong adhesion by grafting phenol groups and in situ esterification. At the same time, the dynamic bonds and covalent bonds in the binder are balanced by regulating the amount of the crosslinking agent, thereby solving the problem that the existing linear polymer binder is prone to bonding failure when subjected to stress, effectively suppressing the volume deformation of the silicon negative electrode during the cycle and improving its electrochemical performance. The nano-silicon negative electrode using the binder of the present invention exhibits high discharge capacity, good rate performance and excellent cycle stability. After 500 cycles at a current density of 2A / g, it can still retain a high capacity of 1738mAh / g and a cycle life of up to 800 cycles. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is the Fourier infrared spectra of the adhesives obtained in Examples 1 to 3 and Comparative Examples 2 to 3.

[0030] Figure 2 These are nanoindentation test, modulus and hardness test graphs of the silicon electrode sheets prepared in Examples 1 to 3 and Comparative Examples 1 to 3.

[0031] Figure 3 It is a diagram of the covalent bond and dynamic supramolecular synergistic action mechanism of the binder of the present invention, and a diagram of the action mechanism of the binder in Comparative Example 1 with only physical cross-linking.

[0032] Figure 4 It is the rate performance of the battery assembled with the negative electrode sheets prepared in Examples 1 to 3 and Comparative Examples 1 to 3.

[0033] Figure 5 It is the electrochemical cycle performance diagram of the battery assembled with the prepared negative electrode sheets obtained in Examples 1 to 3. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0035] Example 1

[0036] This embodiment prepares a negative electrode sheet containing the binder of the present invention and completes its testing process.

[0037] Step 1, preparation of grafted product: hyaluronic acid (HA) with a molecular weight of 400,000 is dissolved in a solvent phosphate buffer (pH 5.5) at a concentration of 10 mg / mL, and after nitrogen deoxygenation at 25°C, 4 2-fold molar equivalents of amidating reagent N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide are added and mixed evenly, and then hyaluronic acid: dopamine is added according to a molar ratio of 1:2 (wherein the amount of phenol groups accounts for the total number of carboxyl groups in the polymer, that is, the dopamine grafting rate is shown in Table 1) The monomer dopamine (DA) containing a phenol group is reacted for 24 hours, wherein. Then, the reaction solution is placed in a dialysis bag, dialyzed with acidic deionized water (pH 5.5) for 72 hours in the dark to remove unreacted substances and phosphates, and then dialyzed in deionized water for 4 hours to remove small molecular impurities. Finally, the grafted product (DAH) is obtained by lyophilization under reduced pressure.

[0038] Step 2, preparation of binder precursor solution: the grafted product and the cross-linking agent iminodiacetic acid (IDA) are mixed in a mass ratio of 2:1 and dissolved in deionized water to prepare a binder precursor solution.

[0039] Step 3, preparation of negative electrode sheet: homogenize nano silicon (negative electrode active material), Super P (conductive additive) and binder precursor solution in a mass ratio of 6:2:2. 2 The uniform slurry is evenly applied on the copper foil, and after heat treatment at 80℃ and 150℃ for 12h and 2h respectively, the negative electrode sheet is sliced ​​to obtain the negative electrode sheet. In this embodiment, the binder is denoted as DAH-c-IDA, and the prepared negative electrode sheet is denoted as Si@DAH-c-IDA.

[0040] Among them, the binder precursor solution undergoes an in-situ thermal crosslinking reaction during the above-mentioned heat treatment process for forming the negative electrode sheet. At this time, the carboxyl group of the crosslinking agent and the hydroxyl group of the high molecular polymer undergo in-situ thermal crosslinking to form a strong covalent ester bond. In this process, the adhesive network formed by the binder, which has both dynamic supramolecular action and ester bond covalent action, is interwoven with the active material (for example, nano silicon particles in this embodiment) and the conductive additive on the silicon negative electrode sheet. The double adhesive network formed by the binder firmly fixes the silicon particles in three dimensions and bears most of the stress generated during the silicon lithiation / delithiation process. Under the action of the binder having a double crosslinking network of dynamic supramolecular action and ester bond covalent action, the mechanical properties of the negative electrode sheet are enhanced, and the problem that the existing linear polymer binder is prone to bonding failure when subjected to stress is solved, and the volume deformation of the silicon negative electrode during the cycle process is effectively suppressed and its electrochemical performance is improved.

[0041] Step 4, negative electrode electrochemical performance test: the prepared negative electrode was transferred into the glove box, and the lithium sheet was used as the counter electrode to assemble a 2025 button cell. The separator was Celgard 2400, and the electrolyte contained 1 mol / L LiPF 6 , dissolved in a mixed solvent of EC / DMC / EMC (1 / 1 / 1, v / v / v), add 5% FEC and 0.5% VC by volume. Seal the assembled battery and let it stand for 12 hours. The static battery is subjected to a constant current electrochemical performance test on a charge and discharge battery test system. Among them, the cycle test is first activated for 3 cycles at a small rate of 0.025C (1C=4A / g), and then a charge and discharge test is performed at 0.2C, with a voltage range of 0.005~1.2V.

[0042] Example 2

[0043] In this embodiment, a negative electrode sheet containing the binder of the present invention and its testing process are prepared, wherein the mass ratio of the grafted product to iminodiacetic acid is 4:1, and the rest of the specific process of the preparation and testing of the negative electrode sheet is carried out with reference to Example 1. In this embodiment, the binder is: DAH 4 I 1 The prepared negative electrode sheet is denoted as: Si@DAH 4 I 1 .

[0044] Example 3

[0045] In this embodiment, a negative electrode sheet containing the binder of the present invention is prepared and tested, wherein the mass ratio of the grafted product to iminodiacetic acid is 1:1, and the rest of the specific process of the negative electrode sheet preparation and testing is carried out with reference to Example 1. In this embodiment, the binder is: DAH 1 I 1 The prepared negative electrode sheet is denoted as: Si@DAH 1 I 1 .

[0046] Example 4

[0047] This embodiment prepares a negative electrode sheet containing the binder of the present invention and a testing process, wherein dopamine is added to react at a molar ratio of hyaluronic acid:dopamine of 1:1, and the rest of the specific process of the negative electrode sheet preparation and testing is carried out with reference to Example 1.

[0048] Example 5

[0049] This embodiment prepares a negative electrode sheet containing the binder of the present invention and a testing process, wherein dopamine is added to react at a molar ratio of hyaluronic acid:dopamine of 1:1.5, and the rest of the specific process of the negative electrode sheet preparation and testing is carried out with reference to Example 1.

[0050] Example 6

[0051] This embodiment prepares a negative electrode sheet containing the binder of the present invention and a testing process, wherein hyaluronic acid with a molecular weight of 200,000 is used for the reaction, and the rest of the specific process of the negative electrode sheet preparation and testing is carried out with reference to Example 1.

[0052] Example 7

[0053] This embodiment prepares a negative electrode sheet containing the binder of the present invention and a testing process, wherein hyaluronic acid with a molecular weight of 600,000 is used for the reaction, and the rest of the specific process of the negative electrode sheet preparation and testing is carried out with reference to Example 1.

[0054] Comparative Example 1

[0055] The binder used in the negative electrode sheet prepared in this comparative example is a mixture of sodium carboxymethyl cellulose and styrene-butadiene rubber in a mass ratio of 1:1, and the rest of the negative electrode sheet preparation process and test process are the same as those in Example 1. The binder in this comparative example is recorded as: CMC-SBR, and the prepared negative electrode sheet is recorded as: Si@CMC-SBR.

[0056] Comparative Example 2

[0057] The negative electrode sheet prepared in this example uses hyaluronic acid as a binder, and the rest of the negative electrode sheet preparation process and test process are the same as in Example 1. The binder in this comparative example is recorded as: HA, and the prepared negative electrode sheet is recorded as: Si@HA.

[0058] Comparative Example 3

[0059] The negative electrode sheet prepared in this example uses the grafted product DAH in Example 1 directly as a binder, and the rest of the negative electrode sheet preparation process and test process are the same as in Example 1. The binder in this comparative example is recorded as: DAH, and the negative electrode sheet prepared is recorded as: Si@DAH.

[0060] Comparative Example 4

[0061] In the negative electrode sheet prepared in this example, the mass ratio of the grafted product to iminodiacetic acid in the binder is 9:1, and the rest of the negative electrode sheet preparation process and test process are the same as in Example 1. The binder in this comparative example is denoted as: DAH 9 I 1 The negative electrode sheet prepared in this comparative example is denoted as: Si@DAH 9 I 1。

[0062] Comparative Example 5

[0063] In the negative electrode sheet prepared in this example, the mass ratio of the grafted product to iminodiacetic acid in the binder is 1:1.5, and the rest of the negative electrode sheet preparation process and test process are the same as in Example 1. The binder in this comparative example is denoted as: DAH 1 I 1.5 The negative electrode sheet prepared in this comparative example is denoted as: Si@DAH 1 I 1.5 .

[0064] The following experiments were conducted to study the binder of the present invention having a chemical and physical dual cross-linked network and the performance of the binder in preparing the silicon negative electrode.

[0065] 1. Structural test of adhesive

[0066] The adhesives of Examples 1 to 3 and the adhesives of Comparative Examples 2 to 3 were subjected to infrared spectroscopy testing. Figure 1 The FTIR spectrum of the HA binder in Comparative Example 2 is 3050-3700 cm -1 、1623cm -1 、1386cm -1 、1042cm -1 The characteristic peaks at correspond to -OH / NH, C=O, CO, -CH 2 OH functional group. The above characteristic peaks can still be observed in the FTIR spectrum of DAH in Comparative Example 3. -1 The characteristic peaks at 1530 cm-1 are attributed to C=O and C=C stretching vibrations. -1 and 3087cm -1 The new peak at 1045 cm corresponds to the NH bending and stretching vibrations in the generated amide bond, while the peak at 1045 cm -1 The peak at -CH 2 The stretching vibrations of OH and CN are related. Compared with the FTIR spectrum of the DAH binder in Comparative Example 3, the DAH in Example 2 4 I 1 The characteristic peaks attributed to C=O are from 1619cm -1 Move to 1631cm -1 A new shoulder peak appeared, while DAH-c-IDA in Example 1 and DAH in Example 3 1 I 1 The corresponding characteristic peaks were moved to higher wave numbers (1714cm -1 and 1718cm -1 ), all of which prove the formation of covalent ester bonds.

[0067] 2. Structure and performance test of silicon negative electrode

[0068] 1. Mechanical properties test

[0069] The mechanical properties of the silicon electrodes prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were evaluated by nanoindentation testing. Figure 2 As shown, the applied load gradually increases to 3 mN and is unloaded after being maintained for a period of time. Si@CMC-SBR electrode (Comparative Example 1), Si@HA electrode (Comparative Example 2), Si@DAH electrode (Comparative Example 3), Si@DAH 4 I 1 electrode (Example 2), Si@DAH-c-IDA electrode (Example 1), Si@DAH 1 I 1 The maximum indentation depths of the electrode (Example 3) at 3 mN were 3630 nm, 3413 nm, 2926 nm, 2413 nm, 2098 nm, and 2738 nm, respectively (e.g. Figure 2 As shown in Figure a). Since the binder in Examples 1 to 3 has a covalent cross-linked structure and a certain energy dissipation capacity, it can withstand the huge stress and strain of Si. Therefore, under the same load, the Si electrodes in Examples 1 to 3 show smaller deformation. In addition, the Si electrodes in Examples 1 to 3 have a larger modulus and hardness (such as Figure 2 Its solid electrode structure can withstand the dramatic volume expansion of silicon and has little deformation under external stress, which is conducive to maintaining the stability of the electrode structure.

[0070] 2. Adhesion test

[0071] Paste the electrode sample coated surface (20mm×60mm) to 3M VHB TM The tape was then pasted onto a stainless steel plate and tested using a universal tensile testing machine at 100 mm min. -1 The 180° peeling test was carried out at a tensile speed of 1.5° to measure the peeling force. The results are shown in Table 1.

[0072] 3. Electrochemical performance test

[0073] The preparation conditions of the binders of Examples 1 to 7 and Comparative Examples 1 to 5, the dopamine grafting ratio, and the binding force and cycle performance at 0.2C of the obtained silicon electrodes are summarized in Table 1.

[0074] Table 1

[0075] From the data comparison in Table 1, it can be seen that the silicon negative electrodes in Examples 1 to 7 have higher stripping forces and better cycle stability, and can retain capacities of 1940 mAh / g, 1807 mAh / g, 1766 mAh / g, 1617 mAh / g, 1670 mAh / g, 1705 mAh / g and 1652 mAh / g respectively after 450 cycles at a current density of 2 A / g. Figure 3 The diagram of the synergistic mechanism of covalent bonds and dynamic supramolecular effects of the present invention in Figure a illustrates that when the binders of Examples 1 to 7 are applied to silicon negative electrodes, under the synergistic effect of the dynamic hydrogen bonds and strong ester bonds of the binders, the huge stress generated by the volume strain of silicon during the cycle is effectively dissipated, thereby maintaining the integrity of the electrode structure. Figure 3 Figure b shows the mechanism of action of only physical crosslinking, taking the binder CMC-SBR in Comparative Example 1 as an example. Since the interaction between CMC-SBR and silicon in Comparative Example 1 is weak, when subjected to stress and strain caused by lithium deintercalation from silicon, the molecular chain is prone to linear slip or even structural damage, the bonding force is low, the silicon electrode capacity decays quickly, and the cycle performance is poor. Although the binder HA in Comparative Example 2 is rich in polar functional groups, as a linear polymer, it is easy to detach from the contact point and slip the molecular chain under repeated expansion and contraction of silicon, and cannot maintain the stability of the electrode structure well, so the electrochemical performance is poor. Comparative Example 3 introduces catechol groups to modify the binder to enhance the dynamic hydrogen bonding effect and increase the contact sites with silicon, which improves the bonding force and the electrochemical performance of the silicon electrode to a certain extent. In Comparative Example 4, the binder is not crosslinked enough to limit the movement of silicon particles to linear slip or even damage, so the performance of the silicon electrode does not achieve the expected effect. The high content of crosslinking agent in the binder in Comparative Example 5 has an adverse effect on its mechanical properties and reduces the adhesion sites, so the bonding force decreases and the performance of the silicon electrode deteriorates. The appropriate degree of crosslinking enables the binder to have excellent mechanical properties, while maintaining appropriate dynamic supramolecular interaction with silicon and three-dimensionally restricting the expansion of silicon particles. It can be seen from the data comparison in Table 1 that the silicon negative electrode binder prepared by the method of the present invention has excellent performance.

[0076] The silicon negative electrode sheets prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were assembled into button cells for rate performance testing. The results are as follows: Figure 4 As shown. It can be seen that compared with comparative examples 1 to 3, the rate performance of the silicon negative electrode in Examples 1 to 3 is improved. This is mainly due to the fact that the strong bonding network in Examples 1 to 3 can three-dimensionally fix the silicon particles and maintain continuous electrical contact between silicon and the conductive agent, thereby obtaining excellent rate performance.

[0077] The silicon negative electrode sheets prepared in Examples 1 to 3 were assembled into button cells and subjected to long-term cycle performance tests at 0.5C. The results are as follows: Figure 5As shown. After 800 cycles, the silicon electrodes in Examples 1 to 3 showed reversible capacities of 864 mAh / g, 670 mAh / g, and 577 mAh / g, respectively. Chemical crosslinking gives the binder excellent mechanical properties while maintaining appropriate dynamic supramolecular interactions with silicon, three-dimensionally restricting the expansion of silicon particles, so the cycle life of the Si electrodes in Examples 1 to 3 reaches 800 cycles. Among them, the battery performance prepared with the binder prepared with dopamine grafted hyaluronic acid and iminodiacetic acid in a mass ratio of 2:1 in Example 1 is the best.

[0078] The above embodiments are used to illustrate the present invention rather than to limit the present invention. Any modification and change made to the present invention within the spirit of the present invention and the protection scope of the claims shall fall within the protection scope of the present invention.

Claims

1. A lithium ion battery silicon negative electrode binder, characterized in that: The adhesive is a cross-linked three-dimensional network adhesive, that is, an adhesive containing a double cross-linked network of chemical cross-linking and physical cross-linking; the chemical cross-linking refers to a cross-linked network containing covalent ester bonds, and the physical cross-linking refers to a cross-linked network containing dynamic supramolecular action sites.

2. The method for preparing a lithium ion battery silicon negative electrode binder according to claim 1, characterized in that: After the high molecular polymer is dissolved in a solvent, a monomer containing a phenol group is grafted thereto through an amidation reaction or an esterification reaction, and then a cross-linking agent is added to carry out a thermal cross-linking reaction.

3. The method for preparing a lithium ion battery silicon negative electrode binder according to claim 2, characterized in that: The preparation steps include: S1. Dissolve the polymer in a solvent, add an amidation reagent and stir thoroughly, then add a monomer containing a phenol group and react for 6 to 48 hours under argon or nitrogen. The reaction process is carried out in the dark and in an anaerobic environment, and the grafted product is obtained by dialysis and freeze-drying; S2, mixing the grafted product and the cross-linking agent in a certain mass ratio and dissolving them in deionized water to prepare a binder precursor solution; S3. The binder precursor solution is heat-treated in a vacuum oven at 120-180° C. for 1-12 hours to perform a thermal crosslinking reaction to obtain the binder.

4. The method for preparing a lithium ion battery silicon negative electrode binder according to claim 3, characterized in that: The high molecular polymer includes at least one of hyaluronic acid, sodium alginate, sodium carboxymethyl cellulose, xanthan gum, peach gum, gellan gum and gum arabic.

5. The method for preparing a lithium ion battery silicon negative electrode binder according to claim 4, characterized in that: The molecular weight of the high molecular polymer is ≥100,000.

6. The method for preparing a lithium ion battery silicon negative electrode binder according to claim 3, characterized in that: The monomer containing a phenol group is at least one of dopamine, 5-hydroxydopamine, gallic acid, tannic acid and derivatives thereof.

7. The method for preparing a lithium ion battery silicon negative electrode binder according to claim 3, characterized in that: The cross-linking agent is at least one of iminodiacetic acid, oxalic acid, malonic acid, tartronic acid, succinic acid, adipic acid, suberic acid and 1,3-acetone dicarboxylic acid.

8. The method for preparing a lithium ion battery silicon negative electrode binder according to claim 3, characterized in that: The usage amounts of the monomer containing phenol groups and the high molecular polymer satisfy that the phenol groups account for 5% to 15% of the total amount of carboxyl groups in the high molecular polymer.

9. The method for preparing a silicon negative electrode binder for a lithium ion battery according to claim 3, characterized in that: The mass ratio of the high molecular weight polymer to the cross-linking agent is 4:1 to 1:

1.

10. The method for preparing a lithium ion battery silicon negative electrode binder according to claim 3, characterized in that: The solvent in step S1 is at least one of deionized water, phosphate buffer, and 4-morpholineethanesulfonic acid buffer with a pH value of ≤7.

11. The method for preparing a silicon negative electrode binder for lithium ion batteries according to claim 3, characterized in that: The amidation reagent in step S1 is at least one of N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and derivatives thereof.

12. A lithium-ion battery silicon negative electrode sheet, characterized in that: The lithium-ion battery silicon negative electrode sheet contains the binder according to claim 1.

13. A method for preparing a lithium-ion battery silicon negative electrode sheet, characterized in that: Includes steps: Weighing the negative electrode active material, the conductive additive and the binder precursor solution prepared in step S2 of claim 3, and mixing the three to form a uniform negative electrode slurry; The negative electrode slurry is coated on the copper foil, dried in a vacuum drying oven at 60-80° C. for 8-12 hours, and then heat treated in a vacuum oven at 120-180° C. for 1-12 hours to obtain the lithium ion battery silicon negative electrode sheet.

14. The method for preparing a lithium-ion battery silicon negative electrode sheet according to claim 13, characterized in that: The mass ratio of the negative electrode active material, the conductive additive and the binder precursor solution is 60-80:10-20:10-20.

15. The method for preparing a lithium-ion battery silicon negative electrode sheet according to claim 13, characterized in that: According to 0.5~1.0mg / cm 2 The negative electrode slurry is coated on the copper foil with an area density of .

16. The method for preparing a lithium-ion battery silicon negative electrode sheet according to claim 13, characterized in that: The negative electrode active material is at least one of nano silicon, micro silicon and silicon-carbon material.

Citation Information

Patent Citations

  • Preparation and application of binder for negative electrode of lithium ion battery based on tannic acid and derivatives thereof

    CN115172752A

  • Silicon-based negative electrode binder with topological three-dimensional structure, negative electrode plate, preparation method of negative electrode plate and battery

    CN117038991A

  • Silicon negative electrode binder with chemical / ionic / hydrogen bond triple cross-linked network and preparation method of silicon negative electrode binder

    CN117050679A

  • Application of self-adaptive three-dimensional conductive binder in silicon-based lithium ion battery

    CN117525425A

  • Self-emulsifying aqueous emulsion binder for silicon-based negative electrode of lithium ion battery and preparation method of self-emulsifying aqueous emulsion binder

    CN117673360A

Cited By

  • Aqueous binder, preparation method and application thereof, and sodium ion battery

    CN120442193A