Children's clothing fabric with moisture absorption and perspiration wicking function and preparation method thereof

Through the preparation of modified fibers, combined with materials such as chitosan, copper chloride, aniline, magnesium hydroxide and acrylonitrile, the problem of insufficient moisture absorption and antibacterial properties of children's textiles is solved, and multiple performance improvements are achieved to ensure children's skin healthy.

CN118814296BActive Publication Date: 2024-11-15GUANGDONG KINGFA MATERNITY & BABY PRODUCTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411295991.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-15
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

Children's textiles lack moisture-wicking and antibacterial properties, which leads to the occurrence of skin diseases. A children's clothing fabric that can both have moisture-wicking and antibacterial properties.

Method used

Modified chitosan is prepared by reacting chitosan with salicylic aldehyde and copper chloride, and polymerization of aniline and 3-aminothiophenyl thiophenol are deposited on the surface of magnesium hydroxide to form polyaniline coated magnesium hydroxide, followed by Polymerized with 1,4-butadiene and 1,3-diallyltetramethyldisilane, then react with methyl iodine to form modified polyaniline coated with magnesium hydroxide, and with acrylonitrile and male The acid anhydride is copolymerized, 7-amino-4-methylcoumarin is introduced to form a modified acrylonitrile copolymer, and is prepared into a spinning liquid for wet spinning.

Benefits of technology

It achieves excellent moisture-absorbing, antibacterial, antistatic, flame-retardant, ultraviolet and mechanical properties of children's clothing fabrics to ensure the health of children's skin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a children's clothing fabric with moisture absorption and perspiration function and a preparation method thereof, and relates to the technical field of textile fabrics. When preparing the children's clothing fabric with moisture absorption and perspiration function, the present invention sequentially reacts chitosan with salicylaldehyde and copper chloride to obtain modified chitosan; 1,4-butanedithiol and 1,3-diallyltetramethyldisilane are polymerized and grown on polyaniline-coated magnesium hydroxide, and then reacted with iodomethane to obtain modified polyaniline-coated magnesium hydroxide; acrylonitrile and maleic anhydride are copolymerized, and then reacted with 7-amino-4-methylcoumarin to obtain a modified acrylonitrile copolymer; modified acrylonitrile copolymer, modified chitosan, and modified polyaniline-coated magnesium hydroxide are prepared into spinning solution, and modified polyacrylonitrile fiber is obtained by wet spinning, and then the modified polyacrylonitrile fiber is woven into a children's clothing fabric with moisture absorption and perspiration function. The children's clothing fabric with moisture absorption and perspiration function prepared by the present invention has excellent flame retardant, UV protection, antistatic, antibacterial and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile fabrics, in particular to a children's clothing fabric with moisture absorption and perspiration discharge functions and a preparation method thereof. Background Art

[0002] Commonly used textiles have no inhibitory effect on bacteria or fungi. The porous structure of textile fiber fabrics provides a carrier for the reproduction of bacteria; the sweat, sebum and other secretions discharged by children in daily activities provide a nutrient source for the reproduction of bacteria. Children's body temperature regulation center is imperfect, they are afraid of heat and sweat easily. If they are not absorbed and sweated in time, bacteria will easily breed on the surface of the skin, causing skin diseases. Therefore, children's clothing fabrics need to have sufficient moisture absorption and sweat removal performance and antibacterial properties to keep children comfortable and healthy and protect their healthy growth. Based on the above problems, it is necessary to provide a children's clothing fabric with moisture absorption and sweat removal function and a preparation method, which can absorb moisture and sweat while being antibacterial to protect the healthy growth of children. Summary of the invention

[0003] The object of the present invention is to provide a children's clothing fabric with moisture absorption and perspiration discharge function and a preparation method thereof, so as to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a children's clothing fabric with moisture absorption and perspiration function, wherein the children's clothing fabric with moisture absorption and perspiration function is prepared by reacting chitosan with salicylaldehyde and cupric chloride in sequence to obtain modified chitosan; polymerizing and depositing aniline and 3-aminobenzenethiol on the surface of magnesium hydroxide to obtain polyaniline-coated magnesium hydroxide; polymerizing and growing 1,4-butanedithiol and 1,3-diallyltetramethyldisilane on the polyaniline-coated magnesium hydroxide, and then reacting with iodomethane to obtain modified polyaniline-coated magnesium hydroxide; copolymerizing acrylonitrile with maleic anhydride, and then reacting with 7-amino-4-methylcoumarin to obtain a modified acrylonitrile copolymer; preparing a spinning solution with the modified acrylonitrile copolymer, modified chitosan, and modified polyaniline-coated magnesium hydroxide, wet spinning to obtain modified polyacrylonitrile fiber, and then weaving the modified polyacrylonitrile fiber into fabric.

[0005] A method for preparing a children's clothing fabric with moisture absorption and perspiration wicking function, comprising the following preparation steps:

[0006] (1) Chitosan, acetic acid, anhydrous ethanol and deionized water are mixed uniformly in a mass ratio of 1:(0.7-0.9):(20-22):(30-34), and salicylaldehyde (2-2.4 times the mass of chitosan) is added dropwise at a uniform rate within 15 minutes at 10-30°C and 300-500 r / min stirring conditions, and the temperature is raised to 55-65°C, and the stirring reaction is continued for 12-14 hours, and the mixture is filtered and dried at 50-60°C under vacuum conditions for 6-7 hours to obtain pre-modified chitosan; the pre-modified chitosan is immersed in a copper chloride solution, ultrasonically vibrated for 3-4 hours, filtered and dried at 50-60°C under vacuum conditions for 8-10 hours to obtain modified chitosan;

[0007] (2) Polyaniline-coated magnesium hydroxide, 1,4-butanedithiol, azobisisobutyronitrile, and toluene are mixed evenly in a mass ratio of 1:(1.5-1.7):(0.03-0.05):(8-10), 1,3-diallyltetramethyldisilane (1.1-1.2 times the molar amount of 1,4-butanedithiol) is added, and the mixture is stirred at 70-80°C and 300-500 r / min for 2-3 hours, filtered, and dried at 50-60°C under vacuum conditions for 7-8 hours. Pre-modified polyaniline-coated magnesium hydroxide is obtained; in a light-proof condition, pre-modified polyaniline-coated magnesium hydroxide, methyl iodide, and N,N-dimethylformamide are mixed uniformly in a mass ratio of 1:(1.3-1.5):(8-10), stirred at 10-30° C. and 300-500 r / min in a light-proof condition for 20-24 hours, filtered, washed with deionized water for 3-5 times, and dried at 50-60° C. under vacuum conditions for 8-10 hours to obtain modified polyaniline-coated magnesium hydroxide;

[0008] (3) Add acrylonitrile and maleic anhydride in a molar ratio of 1:(0.2~0.3) to N,N-dimethylformamide (13~15 times the mass of acrylonitrile) and mix well to prepare a comonomer solution; under a nitrogen atmosphere, at 50~60°C and stirring at 300~500r / min, add the initiator solution dropwise to the comonomer solution at a uniform rate within 25min, continue stirring and reacting for 15~17h, add 3~4 times the volume of the comonomer solution Deionized water, mix evenly, filter, and dry at 50-60°C for 8-10 hours under vacuum conditions to obtain an acrylonitrile copolymer; mix the acrylonitrile copolymer, 7-amino-4-methylcoumarin, and toluene at a mass ratio of 1:(0.4-0.6):(8-10), stir at 50-60°C, 300-500r / min for 3-4 hours, and dry at 50-60°C for 8-10 hours under vacuum conditions to obtain a modified acrylonitrile copolymer;

[0009] (4) Mixing modified acrylonitrile copolymer, modified chitosan, modified polyaniline-coated magnesium hydroxide and N,N-dimethylformamide in a mass ratio of 1:(0.07-0.08):(0.04-0.05):(6-7) uniformly, stirring at 10-30°C and 300-500 r / min for 30-40 min to prepare a spinning solution; wet spinning the spinning solution to obtain modified polyacrylonitrile fiber; and weaving the modified polyacrylonitrile fiber into a children's clothing fabric with moisture absorption and perspiration removal function using a textile machine.

[0010] As an optimization, the chitosan in step (1) has a deacetylation degree of 94% and a molecular weight of 85 kDa.

[0011] As an optimization, the copper chloride solution in step (1) is prepared by uniformly mixing copper chloride, anhydrous ethanol and deionized water in a mass ratio of 1:(2-3):(6-8).

[0012] As an optimization, the polyaniline-coated magnesium hydroxide in step (2) is prepared by mixing magnesium hydroxide, aniline, 3-aminothiophenol, and a 1-2% hydrochloric acid aqueous solution in a mass ratio of 1:(3-4):(1-1.4):(20-24) in a nitrogen atmosphere, and ultrasonically dispersing for 1-2 hours to prepare a mixed solution; in a nitrogen atmosphere, at 0-2°C and 300-500 r / min stirring conditions, uniformly adding the oxidant solution to the mixed solution within 20 minutes, continuing to stir and react for 20-24 hours, filtering, washing with anhydrous ethanol for 3-5 times, and drying at 60-70°C under vacuum conditions for 8-10 hours to obtain the polyaniline-coated magnesium hydroxide.

[0013] As an optimization, the particle size of the magnesium hydroxide is 1.6~2μm.

[0014] As an optimization, the oxidant solution is prepared by uniformly mixing 0.06-0.08 times the mass of aniline with 1-2% hydrochloric acid aqueous solution in a mass ratio of 1:(5-7).

[0015] As an optimization, the initiator solution in step (3) is prepared by uniformly mixing 0.03 to 0.05 times the mass of acrylonitrile with azobisisoheptanenitrile and N,N-dimethylformamide in a mass ratio of 1:(5 to 7).

[0016] As an optimization, the process parameters of the wet spinning in step (4) are as follows: placing the spinning solution in a spinning tank, setting the number of spinneret holes to 50, the hole diameter to 0.1 mm, the spinning temperature to 40-50° C., the spinning speed to 40-60 m / min, using a 40-50% by mass dimethyl sulfoxide aqueous solution as a coagulation bath, extruding nitrogen at a pressure of 0.3 MPa into the coagulation bath, and drying at 70-80° C. for 10-12 h under vacuum conditions.

[0017] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: when preparing the children's clothing fabric with moisture absorption and perspiration wicking function, the present invention sequentially reacts chitosan with salicylaldehyde and copper chloride to obtain modified chitosan; polymerizes and deposits aniline and 3-aminothiophenol on the surface of magnesium hydroxide to obtain polyaniline-coated magnesium hydroxide; polymerizes and grows 1,4-butanedithiol and 1,3-diallyltetramethyldisilane on the polyaniline-coated magnesium hydroxide, and then reacts with iodomethane to obtain modified polyaniline-coated magnesium hydroxide; copolymerizes acrylonitrile with maleic anhydride, and then reacts with 7-amino-4-methylcoumarin to obtain a modified acrylonitrile copolymer; the modified acrylonitrile copolymer, modified chitosan and modified polyaniline-coated magnesium hydroxide are prepared into a spinning solution, wet-spinning is performed to obtain modified polyacrylonitrile fibers, and then the modified polyacrylonitrile fibers are woven into fabrics.

[0018] First, the amino group on chitosan and the aldehyde group on salicylaldehyde undergo Schiff base reaction to obtain pre-modified chitosan, and a salicylaldehyde Schiff base structure is formed on the pre-modified chitosan. The pre-modified chitosan is reacted with copper chloride, and copper ions are complexed on the salicylaldehyde Schiff base structure to obtain modified chitosan. Copper ions have a strong antibacterial effect, which can destroy the cell membrane and cell wall of bacteria, leading to extravasation of cell contents. Copper ions can also cause oxidative stress reactions inside bacteria, damage bacterial DNA, proteins and lipids, thereby leading to physiological dysfunction and cell death of bacteria, and endowing the children's clothing fabric with moisture absorption and perspiration function with excellent antibacterial properties. Chitosan contains a large number of hydrophilic groups, which can absorb, transfer and diffuse sweat discharged from the human body, and quickly transfer it to the surface of the fabric for evaporation, thereby improving the moisture absorption and perspiration performance of the children's clothing fabric with moisture absorption and perspiration function.

[0019] Secondly, aniline and 3-aminothiophenol are oxidatively polymerized and deposited on the surface of magnesium hydroxide to obtain polyaniline-coated magnesium hydroxide; and thiol groups are introduced into the polyaniline-coated magnesium hydroxide; polyaniline is a conductive polymer that can form a conductive path inside the children's clothing fabric with moisture absorption and perspiration function, giving the children's clothing fabric with moisture absorption and perspiration function excellent antistatic properties; magnesium hydroxide has an endothermic effect. When magnesium hydroxide is heated by a heat source, it will undergo a dehydration reaction to generate water vapor and magnesium oxide. This is an endothermic reaction that absorbs a large amount of heat. Magnesium oxide will react with carbides on the surface of the combustion product to generate a stable carbide layer. This carbide layer has good thermal insulation properties and can prevent the combustion product from contacting external oxygen. The surface of magnesium hydroxide is modified to improve the compatibility of magnesium hydroxide with the matrix resin. The polyaniline-coated magnesium hydroxide is polyol-coated with 1,4-butanediol and 1,3-diallyltetramethyldisilane by hydrosilylation, and then reacted with iodomethane to obtain modified polyaniline-coated magnesium hydroxide. Si-O bonds and sulfonium salt structures are introduced into the modified polyaniline-coated magnesium hydroxide. The bond energy of the Si-O bond is much higher than that of the CC bond, and it still has good stability under high temperature conditions, and it is not easy to break the molecular chain, which further improves the flame retardancy of the children's clothing fabric with moisture absorption and perspiration function. The sulfonium salt carries a positive charge and interacts with the negatively charged bacterial membrane, resulting in the death of the bacteria, which further improves the antibacterial properties of the children's clothing fabric with moisture absorption and perspiration function.

[0020] Finally, acrylonitrile and maleic anhydride are copolymerized to obtain an acrylonitrile copolymer, anhydride groups are introduced into the acrylonitrile copolymer, and the anhydride groups on the acrylonitrile copolymer react with the amino groups on 7-amino-4-methylcoumarin to obtain a modified acrylonitrile copolymer, and carboxyl groups and coumarin structures are introduced into the side chains of the modified acrylonitrile copolymer. The coumarin structure has a conjugated π-electron system that can absorb ultraviolet light, thereby giving the children's clothing fabric with moisture absorption and perspiration function excellent ultraviolet protection properties; the carboxyl groups introduced into the side chains of the modified acrylonitrile copolymer can undergo esterification reaction with the hydroxyl groups on the modified chitosan, and can also combine with the sulfonium salt on the modified polyaniline-coated magnesium hydroxide through positive and negative charges to form a cross-linked network, thereby inhibiting the relative slippage of the molecular chains, thereby giving the children's clothing fabric with moisture absorption and perspiration function excellent mechanical properties. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] A method for preparing a children's clothing fabric with a moisture absorption and perspiration-wicking function, the method comprising the following preparation steps:

[0024] (1) Chitosan, acetic acid, anhydrous ethanol and deionized water were mixed in a mass ratio of 1:0.7:20:30, and salicylaldehyde twice the mass of chitosan was added dropwise at a uniform rate within 15 minutes at 10°C and 300 r / min stirring conditions, and the temperature was raised to 55°C, and the stirring reaction was continued for 14 hours, and the mixture was filtered and dried at 50°C under vacuum conditions for 7 hours to obtain pre-modified chitosan; copper chloride, anhydrous ethanol and deionized water were mixed in a mass ratio of 1:2:6 to prepare a copper chloride solution; the pre-modified chitosan was immersed in the copper chloride solution, ultrasonically vibrated for 3 hours, filtered and dried at 50°C under vacuum conditions for 10 hours to obtain modified chitosan;

[0025] (2) Under a nitrogen atmosphere, magnesium hydroxide, aniline, 3-aminothiophenol, and a 1% aqueous hydrochloric acid solution were mixed in a mass ratio of 1:3:1:20, and ultrasonically dispersed for 1 hour to prepare a mixed solution; ammonium persulfate (0.06 times the mass of aniline) and a 1% aqueous hydrochloric acid solution were mixed in a mass ratio of 1:5 to prepare an oxidant solution; under a nitrogen atmosphere, at 0°C and 300 r / min stirring conditions, the oxidant solution was uniformly added dropwise to the mixed solution within 20 minutes, and the stirring reaction was continued for 24 hours, filtered, washed with anhydrous ethanol for 3 times, and dried at 60°C under vacuum conditions for 10 hours to obtain polyaniline-coated magnesium hydroxide; polyaniline-coated magnesium hydroxide, 1,4- Butanedithiol, azobisisobutyronitrile, and toluene are mixed evenly in a mass ratio of 1:1.5:0.03:8, 1,3-diallyltetramethyldisilane (1.1 times the molar amount of 1,4-butanedithiol) is added, and the mixture is stirred at 70°C and 300 r / min for 3 hours, filtered, and dried at 50°C for 8 hours under vacuum conditions to obtain pre-modified polyaniline-coated magnesium hydroxide; under light-proof conditions, pre-modified polyaniline-coated magnesium hydroxide, methyl iodide, and N,N-dimethylformamide are mixed evenly in a mass ratio of 1:1.3:8, stirred at 10°C and 300 r / min for 24 hours under light-proof conditions, filtered, washed with deionized water 3 times, and dried at 50°C for 10 hours under vacuum conditions to obtain modified polyaniline-coated magnesium hydroxide;

[0026] (3) Add acrylonitrile and maleic anhydride in a molar ratio of 1:0.2 to N,N-dimethylformamide (13 times the mass of acrylonitrile) and mix them evenly to prepare a comonomer solution; mix azobisisoheptanenitrile (0.03 times the mass of acrylonitrile) and N,N-dimethylformamide in a mass ratio of 1:5 to prepare an initiator solution; under a nitrogen atmosphere, at 50°C, 300 r / min stirring conditions, drop the initiator solution into the comonomer solution at a uniform speed within 25 minutes, continue stirring and reacting for 15 hours, add deionized water (3 times the volume of the comonomer solution), mix evenly, filter, and dry at 50°C for 10 hours under vacuum conditions to obtain an acrylonitrile copolymer; mix acrylonitrile copolymer, 7-amino-4-methylcoumarin, and toluene in a mass ratio of 1:0.4:8, stir at 50°C, 300 r / min for 4 hours, and dry at 50°C for 10 hours under vacuum conditions to obtain a modified acrylonitrile copolymer;

[0027] (4) Modified acrylonitrile copolymer, modified chitosan, modified polyaniline-coated magnesium hydroxide and N,N-dimethylformamide were mixed uniformly in a mass ratio of 1:0.07:0.04:6, and stirred at 10°C and 300 r / min for 40 min to prepare a spinning solution; the spinning solution was placed in a spinning tank, the spinneret holes were set to 50, the hole diameter was 0.1 mm, the spinning temperature was 40°C, the spinning speed was 40 m / min, and a 40% by mass dimethyl sulfoxide aqueous solution was used as a coagulation bath, and the spinning was carried out by a wet spinning process, and nitrogen with a pressure of 0.3 MPa was used to extrude it into the coagulation bath, and it was dried at 70°C for 12 h under vacuum conditions to obtain modified polyacrylonitrile fiber; the modified polyacrylonitrile fiber was spun into a children's clothing fabric with moisture absorption and perspiration wicking function by a textile machine.

[0028] Example 2

[0029] A method for preparing a children's clothing fabric with a moisture absorption and perspiration-wicking function, the method comprising the following preparation steps:

[0030] (1) Chitosan, acetic acid, anhydrous ethanol and deionized water were mixed in a mass ratio of 1:0.8:21:32, and salicylaldehyde (2.2 times the mass of chitosan) was added dropwise at a constant speed within 15 minutes at 20°C and 400 r / min stirring conditions. The temperature was raised to 60°C, and the stirring reaction was continued for 13 hours. The mixture was filtered and dried at 55°C under vacuum conditions for 6.5 hours to obtain pre-modified chitosan. Copper chloride, anhydrous ethanol and deionized water were mixed in a mass ratio of 1:2.5:7 to prepare a copper chloride solution. The pre-modified chitosan was immersed in the copper chloride solution, ultrasonically vibrated for 3.5 hours, filtered and dried at 55°C under vacuum conditions for 9 hours to obtain modified chitosan.

[0031] (2) Under a nitrogen atmosphere, magnesium hydroxide, aniline, 3-aminothiophenol, and a 1.5% aqueous hydrochloric acid solution were mixed in a mass ratio of 1:3.5:1.2:22, and ultrasonically dispersed for 1.5 hours to prepare a mixed solution; ammonium persulfate (0.07 times the mass of aniline) and a 1.5% aqueous hydrochloric acid solution were mixed in a mass ratio of 1:6 to prepare an oxidant solution; under a nitrogen atmosphere, at 1°C and 400 r / min stirring conditions, the oxidant solution was uniformly added dropwise to the mixed solution within 20 minutes, and the stirring reaction was continued for 22 hours, filtered, washed with anhydrous ethanol 4 times, and dried at 65°C under vacuum conditions for 9 hours to obtain polyaniline-coated magnesium hydroxide; polyaniline-coated magnesium hydroxide, 1, 4-Butanedithiol, azobisisobutyronitrile, and toluene are mixed uniformly in a mass ratio of 1:1.6:0.04:9, 1,3-diallyltetramethyldisilane (1.15 times the molar amount of 1,4-butanedithiol) is added, and the mixture is stirred at 75°C and 400r / min for 2.5h, filtered, and dried at 55°C for 7.5h under vacuum conditions to obtain pre-modified polyaniline-coated magnesium hydroxide; under light-proof conditions, pre-modified polyaniline-coated magnesium hydroxide, methyl iodide, and N,N-dimethylformamide are mixed uniformly in a mass ratio of 1:1.4:9, stirred at 20°C and 400r / min for 22h, filtered, washed with deionized water 4 times, and dried at 55°C for 9h under vacuum conditions to obtain modified polyaniline-coated magnesium hydroxide;

[0032] (3) Add acrylonitrile and maleic anhydride in a molar ratio of 1:0.25 to N,N-dimethylformamide (14 times the mass of acrylonitrile) and mix them evenly to prepare a comonomer solution; mix azobisisoheptanenitrile (0.04 times the mass of acrylonitrile) and N,N-dimethylformamide in a mass ratio of 1:6 to prepare an initiator solution; under a nitrogen atmosphere, at 55°C and 400 r / min stirring conditions, drop the initiator solution into the comonomer solution at a uniform rate within 25 minutes, continue stirring and reacting for 16 hours, add deionized water (3.5 times the volume of the comonomer solution), mix evenly, filter, and dry at 55°C under vacuum conditions for 9 hours to obtain an acrylonitrile copolymer; mix acrylonitrile copolymer, 7-amino-4-methylcoumarin, and toluene in a mass ratio of 1:0.5:9, stir and react at 55°C and 400 r / min for 3.5 hours, and dry at 55°C under vacuum conditions for 9 hours to obtain a modified acrylonitrile copolymer;

[0033] (4) Modified acrylonitrile copolymer, modified chitosan, modified polyaniline-coated magnesium hydroxide and N,N-dimethylformamide were mixed uniformly in a mass ratio of 1:0.075:0.045:6.5, stirred at 20°C and 400 r / min for 35 min to prepare a spinning solution; the spinning solution was placed in a spinning tank, the spinneret holes were set to 50, the hole diameter was 0.1 mm, the spinning temperature was 45°C, the spinning speed was 50 m / min, and a 45% by mass dimethyl sulfoxide aqueous solution was used as a coagulation bath, and the spinning was carried out by a wet spinning process, and nitrogen gas with a pressure of 0.3 MPa was used to extrude the fibers into the coagulation bath, and the fibers were dried at 75°C for 11 h under vacuum conditions to obtain modified polyacrylonitrile fibers; the modified polyacrylonitrile fibers were spun into children's clothing fabrics with moisture absorption and perspiration wicking functions using a textile machine.

[0034] Example 3

[0035] A method for preparing a children's clothing fabric with a moisture absorption and perspiration-wicking function, the method comprising the following preparation steps:

[0036] (1) Chitosan, acetic acid, anhydrous ethanol and deionized water were mixed in a mass ratio of 1:0.9:22:34, and salicylaldehyde (2.4 times the mass of chitosan) was added dropwise at a constant speed within 15 minutes at 30°C and 500 r / min stirring conditions. The temperature was raised to 65°C, and the stirring reaction was continued for 12 hours. The mixture was filtered and dried at 60°C under vacuum conditions for 6 hours to obtain pre-modified chitosan. Copper chloride, anhydrous ethanol and deionized water were mixed in a mass ratio of 1:3:8 to prepare a copper chloride solution. The pre-modified chitosan was immersed in the copper chloride solution, ultrasonically vibrated for 4 hours, filtered and dried at 60°C under vacuum conditions for 8 hours to obtain modified chitosan.

[0037] (2) Under a nitrogen atmosphere, magnesium hydroxide, aniline, 3-aminothiophenol, and a 2% aqueous hydrochloric acid solution were mixed in a mass ratio of 1:4:1.4:24, and ultrasonically dispersed for 2 hours to prepare a mixed solution; ammonium persulfate (0.08 times the mass of aniline) and a 2% aqueous hydrochloric acid solution were mixed in a mass ratio of 1:7 to prepare an oxidant solution; under a nitrogen atmosphere, at 2°C and 500 r / min stirring conditions, the oxidant solution was uniformly added dropwise to the mixed solution within 20 minutes, and the stirring reaction was continued for 20 hours, filtered, washed with anhydrous ethanol 5 times, and dried at 70°C under vacuum conditions for 8 hours to obtain polyaniline-coated magnesium hydroxide; polyaniline-coated magnesium hydroxide, 1,4- Butanedithiol, azobisisobutyronitrile, and toluene are mixed evenly in a mass ratio of 1:1.7:0.05:10, 1,3-diallyltetramethyldisilane (1.2 times the molar amount of 1,4-butanedithiol) is added, and the mixture is stirred at 80°C and 500 r / min for 2 hours, filtered, and dried at 60°C for 7 hours under vacuum conditions to obtain pre-modified polyaniline-coated magnesium hydroxide; under light-proof conditions, pre-modified polyaniline-coated magnesium hydroxide, methyl iodide, and N,N-dimethylformamide are mixed evenly in a mass ratio of 1:1.5:10, stirred at 30°C and 500 r / min for 20 hours under light-proof conditions, filtered, washed with deionized water 5 times, and dried at 60°C for 8 hours under vacuum conditions to obtain modified polyaniline-coated magnesium hydroxide;

[0038] (3) Add acrylonitrile and maleic anhydride in a molar ratio of 1:0.3 to N,N-dimethylformamide (15 times the mass of acrylonitrile) and mix them evenly to prepare a comonomer solution; mix azobisisoheptanenitrile (0.05 times the mass of acrylonitrile) and N,N-dimethylformamide in a mass ratio of 1:7 to prepare an initiator solution; under a nitrogen atmosphere, at 60°C and 500 r / min stirring conditions, add the initiator solution dropwise to the comonomer solution at a uniform rate within 25 minutes, continue stirring and reacting for 15 hours, add deionized water (4 times the volume of the comonomer solution), mix evenly, filter, and dry at 60°C under vacuum conditions for 8 hours to obtain an acrylonitrile copolymer; mix acrylonitrile copolymer, 7-amino-4-methylcoumarin, and toluene in a mass ratio of 1:0.6:10, stir and react at 60°C and 500 r / min for 3 hours, and dry at 60°C under vacuum conditions for 8 hours to obtain a modified acrylonitrile copolymer;

[0039] (4) Modified acrylonitrile copolymer, modified chitosan, modified polyaniline-coated magnesium hydroxide and N,N-dimethylformamide were mixed uniformly in a mass ratio of 1:0.08:0.05:7, stirred at 30°C and 500 r / min for 30 min to prepare a spinning solution; the spinning solution was placed in a spinning tank, the spinneret holes were set to 50, the hole diameter was 0.1 mm, the spinning temperature was 50°C, the spinning speed was 60 m / min, and a 50% by mass dimethyl sulfoxide aqueous solution was used as a coagulation bath, and the spinning was carried out by a wet spinning process, and nitrogen with a pressure of 0.3 MPa was used to extrude it into the coagulation bath, and it was dried at 80°C for 10 h under vacuum conditions to obtain modified polyacrylonitrile fiber; the modified polyacrylonitrile fiber was spun into a children's clothing fabric with moisture absorption and perspiration wicking function by a textile machine.

[0040] Comparative Example 1

[0041] The method for preparing a children's clothing fabric with moisture absorption and perspiration wicking function of Comparative Example 1 is different from that of Example 2 in that step (1) is not performed, and step (4) is modified as follows: modified acrylonitrile copolymer, chitosan, modified polyaniline-coated magnesium hydroxide, and N,N-dimethylformamide are mixed uniformly in a mass ratio of 1:0.075:0.045:6.5, stirred at 20°C and 400 r / min for 35 min, and prepared into a spinning solution; the spinning solution is placed in a spinning tank, the number of spinneret holes is set to 50, the hole diameter is 0.1 mm, the spinning temperature is set to 45°C, the spinning speed is set to 50 m / min, a 45% dimethyl sulfoxide aqueous solution is used as a coagulation bath, a wet spinning process is used for spinning, nitrogen gas with a pressure of 0.3 MPa is used to extrude into the coagulation bath, and the modified polyacrylonitrile fiber is dried at 75°C for 11 h under vacuum conditions to obtain the modified polyacrylonitrile fiber; and the modified polyacrylonitrile fiber is spun into a children's clothing fabric with moisture absorption and perspiration wicking function using a textile machine. The remaining steps are the same as in Example 2.

[0042] Comparative Example 2

[0043] The preparation method of the children's clothing fabric with moisture absorption and perspiration function of Comparative Example 2 is different from that of Example 2 in step (2). Step (2) is modified as follows: in a nitrogen atmosphere, magnesium hydroxide, aniline, 3-aminothiophenol, and a hydrochloric acid aqueous solution with a mass fraction of 1.5% are mixed uniformly in a mass ratio of 1:3.5:1.2:22, and ultrasonically dispersed for 1.5 hours to prepare a mixed solution; ammonium persulfate with a mass fraction of 0.07 times that of aniline and a hydrochloric acid aqueous solution with a mass fraction of 1.5% are mixed uniformly in a mass ratio of 1:6 to prepare an oxidant solution; in a nitrogen atmosphere, under stirring conditions of 1°C and 400r / min, the oxidant solution is uniformly added dropwise to the mixed solution within 20 minutes, the stirring reaction is continued for 22 hours, filtered, washed with anhydrous ethanol 4 times, and dried at 65°C under vacuum conditions for 9 hours to obtain modified polyaniline-coated magnesium hydroxide. The remaining steps are the same as those of Example 2.

[0044] Comparative Example 3

[0045] The preparation method of the children's clothing fabric with moisture absorption and perspiration removal function of comparative example 3 is different from that of example 2 in that step (2) is not performed, and step (4) is modified as follows: the modified acrylonitrile copolymer, modified chitosan, magnesium hydroxide, and N,N-dimethylformamide are uniformly mixed in a mass ratio of 1:0.075:0.045:6.5, and stirred at 20°C and 400 r / min for 35 min to prepare a spinning solution; the spinning solution is placed in a spinning tank, the number of spinneret holes is set to 50, the hole diameter is 0.1 mm, the spinning temperature is 45°C, the spinning speed is 50 m / min, and a 45% dimethyl sulfoxide aqueous solution is used as a coagulation bath, a wet spinning process is used for spinning, nitrogen gas with a pressure of 0.3 MPa is used to extrude it into the coagulation bath, and it is dried at 75°C for 11 h under vacuum conditions to obtain modified polyacrylonitrile fiber; and the modified polyacrylonitrile fiber is spun into a children's clothing fabric with moisture absorption and perspiration removal function by a textile machine. The remaining steps are the same as in Example 2.

[0046] Comparative Example 4

[0047] The preparation method of the children's clothing fabric with moisture absorption and perspiration wicking function of Comparative Example 4 is different from that of Example 2 only in that step (3) is not performed, and step (4) is modified as follows: polyacrylonitrile, modified chitosan, modified polyaniline-coated magnesium hydroxide, and N,N-dimethylformamide are mixed uniformly in a mass ratio of 1:0.075:0.045:6.5, and stirred at 20°C and 400 r / min for 35 min to prepare a spinning solution; the spinning solution is placed in a spinning tank, the number of spinneret holes is set to 50, the hole diameter is 0.1 mm, the spinning temperature is 45°C, the spinning speed is 50 m / min, and a 45% dimethyl sulfoxide aqueous solution is used as a coagulation bath, a wet spinning process is used for spinning, nitrogen gas with a pressure of 0.3 MPa is used to extrude it into the coagulation bath, and it is dried at 75°C for 11 h under vacuum conditions to obtain modified polyacrylonitrile fiber; and the modified polyacrylonitrile fiber is spun into a children's clothing fabric with moisture absorption and perspiration wicking function using a textile machine. The remaining steps are the same as in Example 2.

[0048] Test Example 1

[0049] Flame retardant performance test

[0050] Test method: According to GB / T5454 "Textile Combustion Performance Test Oxygen Index Method", the limiting oxygen index of the embodiment and the comparative example was tested using an oxygen index instrument. The results are shown in Table 1.

[0051]

[0052] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 1, it can be found that the children's clothing fabric with moisture absorption and perspiration function prepared by the present invention has good flame retardant properties.

[0053] By comparison, the limiting oxygen index of Examples 1 to 3 is greater than that of Comparative Examples 2 to 3, indicating that aniline and 3-aminothiophenol are oxidatively polymerized and deposited on the surface of magnesium hydroxide to obtain polyaniline-coated magnesium hydroxide, and a mercapto group is introduced on the polyaniline-coated magnesium hydroxide; 1,4-butanedithiol and 1,3-diallyltetramethyldisilane are polymerized and grown on the polyaniline-coated magnesium hydroxide by hydrosilylation, and then reacted with iodomethane to obtain modified polyaniline-coated magnesium hydroxide, and Si-O bonds are introduced on the modified polyaniline-coated magnesium hydroxide, the bond energy of the Si-O bond is much higher than the bond energy of the CC bond, and the polyaniline-coated magnesium hydroxide still has good stability under high temperature conditions, and is not prone to molecular The chain is broken, which improves the flame retardancy of children's clothing fabrics with moisture absorption and perspiration function; magnesium hydroxide has an endothermic effect. When magnesium hydroxide is heated by a heat source, it will undergo a dehydration reaction to generate water vapor and magnesium oxide. This is an endothermic reaction that absorbs a large amount of heat. Magnesium oxide will react with the carbide on the surface of the combustion product to generate a stable carbide layer. This carbide layer has good thermal insulation properties and can prevent the combustion product from contacting external oxygen. The surface of magnesium hydroxide is modified to improve the compatibility of magnesium hydroxide with the matrix resin, so that magnesium hydroxide is not easy to agglomerate in the matrix resin and is evenly dispersed, thereby giving the children's clothing fabrics with moisture absorption and perspiration function excellent flame retardant properties.

[0054] Test Example 2

[0055] Antimicrobial performance testing

[0056] Test method: The antibacterial performance of the embodiment and the comparative example was analyzed by comparing the number of E. coli colonies cultured in agar medium for 16 hours using the oscillation method GB / T 20944.3. The results are shown in Table 2.

[0057]

[0058] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 2, it can be found that the children's clothing fabric with moisture absorption and perspiration function prepared by the present invention has good antibacterial properties.

[0059] By comparison, the antibacterial rates of Examples 1 to 3 are greater than that of Comparative Example 1, indicating that the amino groups on chitosan and the aldehyde groups on salicylaldehyde undergo Schiff base reaction to obtain pre-modified chitosan, a salicylaldehyde Schiff base structure is formed on the pre-modified chitosan, the pre-modified chitosan reacts with copper chloride, and copper ions are complexed on the salicylaldehyde Schiff base structure to obtain modified chitosan; copper ions have a strong antibacterial effect, can destroy the cell membrane and cell wall of bacteria, and cause extravasation of cell contents, and copper ions can also cause oxidative stress reactions inside bacteria, damage bacterial DNA, proteins and lipids, thereby causing physiological dysfunction and cell death of bacteria, and giving excellent antibacterial properties to the children's clothing fabric with moisture absorption and perspiration function.

[0060] By comparison, the antibacterial rates of Examples 1 to 3 are greater than those of Comparative Examples 2 to 3, indicating that aniline and 3-aminothiophenol are oxidatively polymerized and deposited on the surface of magnesium hydroxide to obtain polyaniline-coated magnesium hydroxide; and thiol groups are introduced on the polyaniline-coated magnesium hydroxide; 1,4-butanedithiol and 1,3-diallyltetramethyldisilane are polymerized and grown on the polyaniline-coated magnesium hydroxide by hydrosilylation, and then reacted with iodomethane to obtain modified polyaniline-coated magnesium hydroxide, and a sulfonium salt structure is introduced on the modified polyaniline-coated magnesium hydroxide, and the sulfonium salt carries a positive charge and interacts with the negatively charged bacterial membrane, resulting in bacterial death, thereby further improving the antibacterial properties of the children's clothing fabric with moisture absorption and perspiration function.

[0061] Test Example 3

[0062] Antistatic performance test

[0063] Test method: According to GB / T 12703, the half-life method is used to discharge the sample placed on the rotating metal platform with a 10KV high voltage for 30 seconds. When the static voltage is stable, the time and half-life when the induced voltage decays to half are detected. The antistatic effects of the embodiments and comparative examples are evaluated based on the half-life. The results are shown in Table 3.

[0064]

[0065] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 3, it can be found that the children's clothing fabric with moisture absorption and perspiration function prepared by the present invention has good antistatic performance.

[0066] By comparison, the half-lives of Examples 1 to 3 are shorter than the half-life of Comparative Example 3, indicating that aniline and 3-aminothiophenol are oxidatively polymerized and deposited on the surface of magnesium hydroxide to obtain polyaniline-coated magnesium hydroxide; polyaniline is a conductive polymer that can form a conductive path inside the children's clothing fabric with moisture absorption and perspiration function, thereby giving the children's clothing fabric with moisture absorption and perspiration function excellent antistatic properties.

[0067] Test Example 4

[0068] UV resistance and mechanical properties testing

[0069] Test method: The mechanical properties of the polyacrylonitrile fibers prepared in the embodiment and the comparative example were tested using an XL-1A filament tensile tester. The sample was passed around the yarn guide hook and the yarn guide wheel, and passed downward through the upper and lower clamps to ensure that the sample was straightened without relaxation. A pre-tension of about 10 cN was applied to the sample. The lower clamp drove the sample downward until the sample broke and then returned to its original position to obtain the breaking strength of the sample. After that, the original sample without the breaking test was irradiated with a xenon arc lamp for 72 hours, and then its breaking strength was tested by the same method. The breaking strength change rate of the embodiment and the comparative example before and after the ultraviolet aging treatment was calculated. The breaking strength change rate = (original breaking strength of the sample - breaking strength after ultraviolet aging treatment) / original breaking strength of the sample × 100%. The results are shown in Table 4.

[0070]

[0071] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 4, it can be found that the children's clothing fabric with moisture absorption and perspiration function prepared by the present invention has good UV protection and mechanical properties.

[0072] By comparison, the fracture strength of Examples 1 to 3 is greater than that of Comparative Examples 2 to 4, indicating that aniline and 3-aminothiophenol are oxidatively polymerized and deposited on the surface of magnesium hydroxide to obtain polyaniline-coated magnesium hydroxide; and a mercapto group is introduced on the polyaniline-coated magnesium hydroxide; 1,4-butanedithiol and 1,3-diallyltetramethyldisilane are polymerized and grown on the polyaniline-coated magnesium hydroxide by hydrosilylation, and then reacted with iodomethane to obtain modified polyaniline-coated magnesium hydroxide, and a sulfonium salt structure is introduced on the modified polyaniline-coated magnesium hydroxide; acrylonitrile and maleic anhydride are copolymerized to obtain an acrylonitrile copolymer, an anhydride group is introduced on the acrylonitrile copolymer, and the anhydride group on the acrylonitrile copolymer reacts with 7- The amino group on amino-4-methylcoumarin is reacted to obtain a modified acrylonitrile copolymer, and a carboxyl group is introduced into the side chain of the modified acrylonitrile copolymer; the modified acrylonitrile copolymer, modified chitosan, and modified polyaniline-coated magnesium hydroxide are prepared into a spinning solution, and modified polyacrylonitrile fiber is obtained by wet spinning, and then the modified polyacrylonitrile fiber is spun into a children's clothing fabric with moisture absorption and perspiration function; the carboxyl group introduced on the side chain of the modified acrylonitrile copolymer can undergo an esterification reaction with the hydroxyl group on the modified chitosan, and can also combine with the sulfonium salt on the modified polyaniline-coated magnesium hydroxide through positive and negative charges to form a cross-linked network, inhibit the relative slip of the molecular chain, and give the children's clothing fabric with moisture absorption and perspiration function excellent mechanical properties.

[0073] By comparison, the breaking strength change rate of Examples 1 to 3 is less than that of Comparative Example 4, indicating that acrylonitrile and maleic anhydride are copolymerized to obtain an acrylonitrile copolymer, an anhydride group is introduced into the acrylonitrile copolymer, the anhydride group on the acrylonitrile copolymer reacts with the amino group on 7-amino-4-methylcoumarin to obtain a modified acrylonitrile copolymer, a coumarin structure is introduced into the side chain of the modified acrylonitrile copolymer, and the coumarin structure has a conjugated π electron system, which can absorb ultraviolet light, thereby giving the children's clothing fabric with moisture absorption and perspiration function excellent anti-ultraviolet performance.

[0074] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a children's clothing fabric with moisture absorption and perspiration wicking function, characterized in that: The method for preparing the children's clothing fabric with moisture absorption and perspiration wicking function comprises the following preparation steps: (1) Chitosan, acetic acid, anhydrous ethanol and deionized water are mixed uniformly in a mass ratio of 1:(0.7-0.9):(20-22):(30-34), and salicylaldehyde (2-2.4 times the mass of chitosan) is added dropwise at a uniform rate within 15 minutes at 10-30°C and 300-500 r / min stirring conditions, and the temperature is raised to 55-65°C, and the stirring reaction is continued for 12-14 hours, and the mixture is filtered and dried at 50-60°C under vacuum conditions for 6-7 hours to obtain pre-modified chitosan; the pre-modified chitosan is immersed in a copper chloride solution, ultrasonically vibrated for 3-4 hours, filtered and dried at 50-60°C under vacuum conditions for 8-10 hours to obtain modified chitosan; (2) Under a nitrogen atmosphere, magnesium hydroxide, aniline, 3-aminothiophenol, and a 1-2% aqueous hydrochloric acid solution are mixed in a mass ratio of 1:(3-4):(1-1.4):(20-24), and ultrasonically dispersed for 1-2 hours to prepare a mixed solution; under a nitrogen atmosphere, at 0-2°C and 300-500 r / min stirring conditions, the oxidant solution is uniformly added dropwise to the mixed solution within 20 minutes, and the stirring reaction is continued for 20-24 hours, filtered, washed with anhydrous ethanol for 3-5 times, and dried at 60-70°C under vacuum conditions for 8-10 hours to obtain polyaniline-coated magnesium hydroxide; polyaniline-coated magnesium hydroxide, 1,4-butanedithiol, azobisisobutyronitrile, and toluene are mixed in a mass ratio of 1:(1.5-1.7):(0.03-0.0 5): (8~10) mix evenly, add 1,3-diallyltetramethyldisilane with a molar amount of 1.1~1.2 times of 1,4-butanedithiol, stir and react at 70~80℃, 300~500r / min for 2~3h, filter, and dry at 50~60℃ for 7~8h under vacuum conditions to obtain pre-modified polyaniline-coated magnesium hydroxide; under light-proof conditions, mix pre-modified polyaniline-coated magnesium hydroxide, iodomethane, and N,N-dimethylformamide in a mass ratio of 1: (1.3~1.5): (8~10) evenly, stir and react at 10~30℃, 300~500r / min in a light-proof manner for 20~24h, filter, wash with deionized water 3~5 times, and dry at 50~60℃ for 8~10h under vacuum conditions to obtain modified polyaniline-coated magnesium hydroxide; (3) Add acrylonitrile and maleic anhydride in a molar ratio of 1:(0.2~0.3) to N,N-dimethylformamide (13~15 times the mass of acrylonitrile) and mix well to prepare a comonomer solution; under a nitrogen atmosphere, at 50~60°C and stirring at 300~500r / min, add the initiator solution dropwise to the comonomer solution at a uniform rate within 25min, continue stirring and reacting for 15~17h, add 3~4 times the volume of the comonomer solution Deionized water, mix evenly, filter, and dry at 50-60°C for 8-10 hours under vacuum conditions to obtain an acrylonitrile copolymer; mix the acrylonitrile copolymer, 7-amino-4-methylcoumarin, and toluene at a mass ratio of 1:(0.4-0.6):(8-10), stir at 50-60°C, 300-500r / min for 3-4 hours, and dry at 50-60°C for 8-10 hours under vacuum conditions to obtain a modified acrylonitrile copolymer; (4) uniformly mixing the modified acrylonitrile copolymer, modified chitosan, modified polyaniline-coated magnesium hydroxide, and N,N-dimethylformamide in a mass ratio of 1:(0.07-0.08):(0.04-0.05):(6-7), stirring at 10-30° C. and 300-500 r / min for 30-40 min to prepare a spinning solution; wet spinning the spinning solution to obtain modified polyacrylonitrile fiber; Modified polyacrylonitrile fiber is spun into children's clothing fabric with moisture absorption and perspiration wicking function by using a textile machine.

2. The method for preparing a children's clothing fabric with moisture absorption and perspiration wicking function according to claim 1, characterized in that: The chitosan in step (1) has a deacetylation degree of 94% and a molecular weight of 85 kDa.

3. The method for preparing a children's clothing fabric with moisture absorption and perspiration wicking function according to claim 1, characterized in that: The copper chloride solution in step (1) is prepared by uniformly mixing copper chloride, anhydrous ethanol and deionized water in a mass ratio of 1:(2-3):(6-8).

4. The method for preparing a children's clothing fabric with moisture absorption and perspiration wicking function according to claim 1, characterized in that: The particle size of the magnesium hydroxide in step (2) is 1.6-2 μm.

5. The method for preparing a children's clothing fabric with moisture absorption and perspiration wicking function according to claim 1, characterized in that: The oxidant solution in step (2) is prepared by uniformly mixing 0.06-0.08 times the mass of aniline with 1-2% hydrochloric acid aqueous solution in a mass ratio of 1:(5-7).

6. The method for preparing a children's clothing fabric with moisture absorption and perspiration wicking function according to claim 1, characterized in that: The initiator solution in step (3) is prepared by uniformly mixing 0.03 to 0.05 times the mass of acrylonitrile with azobisisoheptanenitrile and N,N-dimethylformamide in a mass ratio of 1:(5 to 7).

7. The method for preparing a children's clothing fabric with moisture absorption and perspiration wicking function according to claim 1, characterized in that: The process parameters of the wet spinning in step (4) are as follows: placing the spinning solution in a spinning tank, setting the number of spinneret holes to 50, the hole diameter to 0.1 mm, the spinning temperature to 40-50° C., the spinning speed to 40-60 m / min, using a 40-50% by mass dimethyl sulfoxide aqueous solution as a coagulation bath, extruding nitrogen at a pressure of 0.3 MPa into the coagulation bath, and drying at 70-80° C. for 10-12 h under vacuum conditions.

8. A children's clothing fabric with moisture absorption and perspiration removal function prepared by the method for preparing a children's clothing fabric with moisture absorption and perspiration removal function according to any one of claims 1 to 7.