A flocculant containing modified L-arginine and preparation method thereof
A modified L-arginine flocculant was prepared by combining chitosan-modified L-arginine modified polyurethane, quaternary ammonium modified fluorine-containing epoxy resin, polyacrylamide and aluminum trichloride. The problem of poor flocculation effect of traditional flocculants has been solved, the flocculation effect has been significantly improved, and the efficiency of the water treatment process has been enhanced.
Patent Information
- Application Number
- CN202411310402.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-20
AI Technical Summary
The poor flocculation effect of traditional flocculants hinders its further application and development in water treatment.
Using a flocculant containing modified L-arginine, a combination of L-arginine modified polyurethane, quaternary ammonium salt modified fluorine-containing epoxy resin, polyacrylamide and aluminum trichloride , improve the flocculation effect of flocculant through specific preparation methods.
The flocculation effect of the flocculant is significantly improved, and it can more effectively accumulate and settle suspended particles and colloidal substances in the water treatment process, which improves the efficiency of the water treatment process.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flocculants, in particular to a flocculant containing modified L-arginine and a preparation method thereof. Background Art
[0002] Flocculant is a chemical agent used in water treatment, which aims to promote the aggregation of suspended particles in water to form larger flocs, so as to facilitate subsequent treatment processes such as precipitation and filtration. It plays an important role in the water treatment process by adsorbing particles and "building bridges" between particles to promote aggregation and achieve solid-liquid separation. However, the flocculation effect of traditional flocculants is poor, which hinders their further application and development. Therefore, how to avoid this phenomenon is the key to solving the problem. For example, the rapid flocculant published in patent CN101786701A has the characteristics of wide applicability, fast flocculation, energy saving and environmental protection, but its flocculation effect needs to be improved. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies of the prior art, the present invention provides a flocculant containing modified L-arginine and a preparation method thereof, which has good flocculation effect.
[0005] (II) Technical solution
[0006] To achieve the above object, the present invention provides the following technical solution: a flocculant containing modified L-arginine, comprising the following components by weight: 24-28 parts by weight of chitosan-modified L-arginine-modified polyurethane, 16-20 parts by weight of quaternary ammonium salt-modified fluorine-containing epoxy resin, 10-14 parts by weight of polyacrylamide, and 4-8 parts by weight of aluminum chloride;
[0007] Preferably, the preparation method of the chitosan-modified L-arginine-modified polyurethane is:
[0008] (1) Add chitosan to deionized water, stir to dissolve, add a mixed solution of thioglycolic acid and 1-ethyl-(3-dimethylaminopropyl)carbodiimide condensation agent, adjust the pH to 4-6, heat in a water bath, filter, wash and dry after the reaction is completed to obtain intermediate 1;
[0009] (2) adding intermediate 1 to N,N-dimethylformamide solvent, stirring and dispersing, adding divinyl glycol and benzoin dimethyl ether photoinitiator, irradiating with 365 nm ultraviolet light at 25-40° C., centrifuging, washing and drying to obtain intermediate 2;
[0010] (3) adding intermediate 2, L-arginine and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, stirring and mixing, reacting at 45-65°C for 2-4h, and after the reaction, vacuum distilling and drying to obtain chitosan-modified L-arginine chain extender;
[0011] (4) Add fluoroketone diisocyanate and polyoxypropylene glycol to the reactor, then add dibutyltin dilaurate, introduce nitrogen protection, and carry out prepolymerization at 85-90°C for 2.5-3 hours. Then add chitosan-modified L-arginine chain extender to carry out chain extension reaction for 0.5-1.5 hours. After the reaction is completed, cool, wash and dry to obtain chitosan-modified L-arginine modified polyurethane.
[0012] Preferably, the heating temperature in (1) is 35-45° C. and the heating time is 3.5-4 h.
[0013] Preferably, the ultraviolet light irradiation time in (2) is 2.5-3 hours.
[0014] Preferably, the mass ratio of the intermediate 2, L-arginine, and p-toluenesulfonic acid catalyst in (3) is 1:0.8-1.2:0.03-0.05.
[0015] Preferably, the mass ratio of fluoroquinone diisocyanate, polyoxypropylene glycol, dibutyltin dilaurate, and chitosan-modified L-arginine chain extender in (4) is 1:1.3-1.5:0.02-0.03:0.7-0.9.
[0016] Preferably, the preparation method of the quaternary ammonium salt modified fluorine-containing epoxy resin is:
[0017] S1. Add 2-fluoro-phenylalanine and cyanuric acid epoxy resin to N,N-dimethylformamide solvent, react at 32-40°C for 1.2-2h, filter, wash and dry to obtain intermediate 3;
[0018] S2. Add intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, introduce nitrogen protection, react at 80-100°C for 3.5-5.5h, and after the reaction is completed, cool, wash and dry to obtain intermediate 4;
[0019] S3. Add intermediate 4 and bromoethanol to tetrahydrofuran solvent, stir and mix, react at 85-95° C. for 6-8 hours, and after the reaction is completed, cool, wash and dry to obtain a quaternary ammonium salt-modified fluorine-containing epoxy resin.
[0020] Preferably, the mass ratio of 2-fluoro-phenylalanine to cyanuric acid epoxy resin in S1 is 1:1.3-1.34.
[0021] Preferably, the mass ratio of the intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid in S2 is 1:0.85-0.9:0.02-0.05.
[0022] Preferably, the mass ratio of the intermediate 4 to bromoethanol in S3 is 1:0.9-0.95.
[0023] Preferably, the preparation method of the flocculant containing modified L-arginine is: adding chitosan-modified L-arginine-modified polyurethane, quaternary ammonium salt-modified fluorinated epoxy resin, polyacrylamide, and aluminum chloride into a reactor, stirring at a speed of 1200-1300 rpm for 5-10 minutes to obtain a flocculant containing modified L-arginine.
[0024] 3. Beneficial technical effects
[0025] The invention obtains a flocculant containing modified L-arginine by adding chitosan-modified L-arginine-modified polyurethane, quaternary ammonium salt-modified fluorine-containing epoxy resin, polyacrylamide and aluminum chloride into a reactor for stirring.
[0026] The hydroxyl group in chitosan reacts with the carboxyl group in thioglycolic acid to introduce a thiol group to obtain intermediate 1. The thiol group in intermediate 1 reacts with the carbon-carbon double bond in divinyl glycol to introduce a hydroxyl group to obtain intermediate 2. The hydroxyl group in intermediate 2 reacts with the carboxyl group in L-arginine to obtain a chitosan-modified L-arginine chain extender. Fluorone diisocyanate and polyoxypropylene glycol undergo a chain extension reaction under the action of the chitosan-modified L-arginine chain extender to obtain chitosan-modified L-arginine modified polyurethane. The epoxy group in cyanuric acid epoxy resin reacts with the amino group in 2-fluoro-phenylalanine to introduce fluorine and carboxyl groups to obtain intermediate 3. The carboxyl group in intermediate 3 reacts with the hydroxyl group in 3-hydroxy-N,N-diethylaniline to introduce a tertiary amine to obtain intermediate 4. Intermediate 4 reacts with bromoethanol to undergo a quaternization reaction and simultaneously introduces a hydroxyl group to obtain a quaternary ammonium salt-modified fluorinated epoxy resin.
[0027] The high molecular structure of chitosan gives it good adsorption properties and can remove organic matter in water by physical adsorption; sulfur can provide additional adsorption sites in flocculants, enhancing the adsorption capacity for suspended particles and colloidal substances; L-arginine can enhance the bridging effect of organic polymer flocculants, promote the flocculants to form larger flocs, and thus accelerate the sedimentation process; quaternary ammonium salt-modified fluorinated epoxy resin can promote the bridging effect between particles during the flocculation process. Through its macromolecular structure, the epoxy resin molecular chain can simultaneously adsorb multiple suspended particles, causing them to aggregate into larger flocs, thereby accelerating the sedimentation process; quaternary ammonium salts dissociate in water to produce positively charged quaternary ammonium ions that can undergo charge neutralization reactions with negatively charged suspended particles or colloidal particles, thereby reducing their surface charge and causing the particles to aggregate and settle; the negatively charged hydroxyl groups in the flocculant can interact with positively charged impurity particles in the water, promoting their aggregation and precipitation. DETAILED DESCRIPTION Example 1
[0028] (1) chitosan was added to deionized water and stirred to dissolve, and a mixed solution of thioglycolic acid and 1-ethyl-(3-dimethylaminopropyl)carbodiimide condensation agent was added thereto, the pH was adjusted to 4, and the mixture was heated in a water bath at a temperature of 35° C. for 3.5 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain intermediate 1;
[0029] (2) Add intermediate 1 to N,N-dimethylformamide solvent, stir and disperse, then add divinyl glycol and benzoin dimethyl ether photoinitiator, irradiate with 365nm ultraviolet light at 25°C for 2.5h, centrifuge, wash and dry to obtain intermediate 2;
[0030] (3) adding intermediate 2, L-arginine and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 2, L-arginine and p-toluenesulfonic acid catalyst is 1:0.8:0.03, stirring and mixing, reacting at 45°C for 2h, and after the reaction is completed, distilling under reduced pressure and drying to obtain chitosan modified L-arginine chain extender;
[0031] (4) Add fluoroketone diisocyanate and polyoxypropylene glycol to the reactor, then add dibutyltin dilaurate, introduce nitrogen protection, carry out prepolymerization at 85°C, the prepolymerization time is 2.5 hours, and then add chitosan-modified L-arginine chain extender to carry out chain extension reaction, wherein the mass ratio of fluoroketone diisocyanate, polyoxypropylene glycol, dibutyltin dilaurate, and chitosan-modified L-arginine chain extender is 1:1.3:0.02:0.7, the reaction time is 0.5 hours, after the reaction is completed, cool, wash and dry to obtain chitosan-modified L-arginine modified polyurethane;
[0032] (5) Add 2-fluoro-phenylalanine and cyanuric acid epoxy resin to N,N-dimethylformamide solvent, wherein the mass ratio of 2-fluoro-phenylalanine to cyanuric acid epoxy resin is 1:1.3, and react at 32°C for 1.2 h. After the reaction is completed, filter, wash and dry to obtain intermediate 3;
[0033] (6) Add intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid is 1:0.85:0.02, pass nitrogen protection, react at 80°C for 3.5h, and after the reaction is completed, cool, wash and dry to obtain intermediate 4;
[0034] (7) adding intermediate 4 and bromoethanol to tetrahydrofuran solvent, wherein the mass ratio of intermediate 4 to bromoethanol is 1:0.9, stirring and mixing, reacting at 85° C. for 6 h, cooling after the reaction, washing and drying to obtain a quaternary ammonium salt modified fluorine-containing epoxy resin;
[0035] (8) 24 parts by weight of chitosan-modified L-arginine-modified polyurethane, 16 parts by weight of quaternary ammonium salt-modified fluorinated epoxy resin, 10 parts by weight of polyacrylamide, and 4 parts by weight of aluminum chloride were added into a reactor and stirred at a speed of 1200 rpm for 5 minutes to obtain a flocculant containing modified L-arginine. Example 2
[0036] (1) Add chitosan to deionized water, stir to dissolve, add a mixed solution of thioglycolic acid and 1-ethyl-(3-dimethylaminopropyl)carbodiimide condensation agent, adjust the pH to 6, heat in a water bath, wherein the heating temperature is 45° C., the heating time is 4 h, after the reaction is completed, filter, wash and dry to obtain intermediate 1;
[0037] (2) Add intermediate 1 to N,N-dimethylformamide solvent, stir and disperse, then add divinyl glycol and benzoin dimethyl ether photoinitiator, irradiate with 365nm ultraviolet light at 40°C for 3h, centrifuge, wash and dry to obtain intermediate 2;
[0038] (3) adding intermediate 2, L-arginine and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 2, L-arginine and p-toluenesulfonic acid catalyst is 1:1.2:0.05, stirring and mixing, reacting at 65°C for 4 hours, and after the reaction is completed, distilling under reduced pressure and drying to obtain chitosan-modified L-arginine chain extender;
[0039] (4) Add fluoroketone diisocyanate and polyoxypropylene glycol to the reactor, then add dibutyltin dilaurate, introduce nitrogen protection, carry out prepolymerization at 90°C for 3 hours, then add chitosan-modified L-arginine chain extender to carry out chain extension reaction, wherein the mass ratio of fluoroketone diisocyanate, polyoxypropylene glycol, dibutyltin dilaurate and chitosan-modified L-arginine chain extender is 1:1.5:0.03:0.9, the reaction time is 1.5 hours, after the reaction is completed, cool, wash and dry to obtain chitosan-modified L-arginine modified polyurethane;
[0040] (5) Add 2-fluoro-phenylalanine and cyanuric acid epoxy resin to N,N-dimethylformamide solvent, wherein the mass ratio of 2-fluoro-phenylalanine to cyanuric acid epoxy resin is 1:1.34, and react at 40°C for 2 h. After the reaction is completed, filter, wash and dry to obtain intermediate 3;
[0041] (6) Add intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid is 1:0.9:0.05, pass nitrogen protection, react at 100°C for 5.5h, and after the reaction is completed, cool, wash and dry to obtain intermediate 4;
[0042] (7) adding intermediate 4 and bromoethanol to tetrahydrofuran solvent, wherein the mass ratio of intermediate 4 to bromoethanol is 1:0.95, stirring and mixing, reacting at 95° C. for 8 h, cooling after the reaction, washing and drying to obtain a quaternary ammonium salt modified fluorinated epoxy resin;
[0043] (8) 28 parts by weight of chitosan-modified L-arginine-modified polyurethane, 20 parts by weight of quaternary ammonium salt-modified fluorinated epoxy resin, 14 parts by weight of polyacrylamide, and 8 parts by weight of aluminum chloride were added into a reactor and stirred at a speed of 1300 rpm for 10 min to obtain a flocculant containing modified L-arginine. Example 3
[0044] (1) chitosan was added to deionized water and stirred to dissolve, and a mixed solution of thioglycolic acid and 1-ethyl-(3-dimethylaminopropyl)carbodiimide condensation agent was added thereto, the pH was adjusted to 5, and the mixture was heated in a water bath at 40° C. for 3.8 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain intermediate 1;
[0045] (2) Add intermediate 1 to N,N-dimethylformamide solvent, stir and disperse, then add divinyl glycol and benzoin dimethyl ether photoinitiator, irradiate with 365nm ultraviolet light at 32°C for 2.7h, centrifuge, wash and dry to obtain intermediate 2;
[0046] (3) adding intermediate 2, L-arginine and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 2, L-arginine and p-toluenesulfonic acid catalyst is 1:1:0.04, stirring and mixing, reacting at 55°C for 3 hours, and after the reaction is completed, distilling under reduced pressure and drying to obtain chitosan-modified L-arginine chain extender;
[0047] (4) Add fluoroketone diisocyanate and polyoxypropylene glycol to the reactor, then add dibutyltin dilaurate, introduce nitrogen protection, carry out prepolymerization at 87°C, the prepolymerization time is 2.8 hours, and then add chitosan-modified L-arginine chain extender to carry out chain extension reaction, wherein the mass ratio of fluoroketone diisocyanate, polyoxypropylene glycol, dibutyltin dilaurate, and chitosan-modified L-arginine chain extender is 1:1.4:0.025:0.8, the reaction time is 1 hour, after the reaction is completed, cool, wash and dry to obtain chitosan-modified L-arginine modified polyurethane;
[0048] (5) Add 2-fluoro-phenylalanine and cyanuric acid epoxy resin to N,N-dimethylformamide solvent, wherein the mass ratio of 2-fluoro-phenylalanine to cyanuric acid epoxy resin is 1:1.32, and react at 36°C for 1.6 hours. After the reaction is completed, filter, wash and dry to obtain intermediate 3;
[0049] (6) Add intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid is 1:0.87:0.035, pass nitrogen protection, react at 90°C for 4.5h, and after the reaction is completed, cool, wash and dry to obtain intermediate 4;
[0050] (7) adding intermediate 4 and bromoethanol to tetrahydrofuran solvent, wherein the mass ratio of intermediate 4 to bromoethanol is 1:0.92, stirring and mixing, reacting at 90° C. for 7 h, cooling after the reaction, washing and drying to obtain a quaternary ammonium salt modified fluorine-containing epoxy resin;
[0051] (8) 26 parts by weight of chitosan-modified L-arginine-modified polyurethane, 18 parts by weight of quaternary ammonium salt-modified fluorinated epoxy resin, 12 parts by weight of polyacrylamide, and 6 parts by weight of aluminum chloride were added into a reactor and stirred at a speed of 1250 rpm for 8 min to obtain a flocculant containing modified L-arginine. Example 4
[0052] (1) chitosan was added to deionized water and stirred to dissolve, and a mixed solution of thioglycolic acid and 1-ethyl-(3-dimethylaminopropyl)carbodiimide condensation agent was added thereto, the pH was adjusted to 4, and the mixture was heated in a water bath at a temperature of 35° C. for 3.5 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain intermediate 1;
[0053] (2) Add intermediate 1 to N,N-dimethylformamide solvent, stir and disperse, then add divinyl glycol and benzoin dimethyl ether photoinitiator, irradiate with 365nm ultraviolet light at 25°C for 2.5h, centrifuge, wash and dry to obtain intermediate 2;
[0054] (3) adding intermediate 2, L-arginine and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 2, L-arginine and p-toluenesulfonic acid catalyst is 1:0.8:0.03, stirring and mixing, reacting at 45°C for 2h, and after the reaction is completed, distilling under reduced pressure and drying to obtain chitosan modified L-arginine chain extender;
[0055] (4) Add fluoroketone diisocyanate and polyoxypropylene glycol to the reactor, then add dibutyltin dilaurate, introduce nitrogen protection, carry out prepolymerization at 90°C for 3 hours, then add chitosan-modified L-arginine chain extender to carry out chain extension reaction, wherein the mass ratio of fluoroketone diisocyanate, polyoxypropylene glycol, dibutyltin dilaurate and chitosan-modified L-arginine chain extender is 1:1.5:0.03:0.9, the reaction time is 1.5 hours, after the reaction is completed, cool, wash and dry to obtain chitosan-modified L-arginine modified polyurethane;
[0056] (5) Add 2-fluoro-phenylalanine and cyanuric acid epoxy resin to N,N-dimethylformamide solvent, wherein the mass ratio of 2-fluoro-phenylalanine to cyanuric acid epoxy resin is 1:1.34, and react at 40°C for 2 h. After the reaction is completed, filter, wash and dry to obtain intermediate 3;
[0057] (6) Add intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, wherein the mass ratio of intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid is 1:0.9:0.05, pass nitrogen protection, react at 100°C for 5.5h, and after the reaction is completed, cool, wash and dry to obtain intermediate 4;
[0058] (7) adding intermediate 4 and bromoethanol to tetrahydrofuran solvent, wherein the mass ratio of intermediate 4 to bromoethanol is 1:0.92, stirring and mixing, reacting at 90° C. for 7 h, cooling after the reaction, washing and drying to obtain a quaternary ammonium salt modified fluorine-containing epoxy resin;
[0059] (8) 26 parts by weight of chitosan-modified L-arginine-modified polyurethane, 18 parts by weight of quaternary ammonium salt-modified fluorinated epoxy resin, 12 parts by weight of polyacrylamide, and 6 parts by weight of aluminum chloride were added into a reactor and stirred at a speed of 1250 rpm for 8 min to obtain a flocculant containing modified L-arginine.
[0060] Comparative Example 1
[0061] Compared with Example 4, the difference in this comparative example is that chitosan-modified L-arginine-modified polyurethane is not added.
[0062] Comparative Example 2
[0063] Compared with Example 4, the difference in this comparative example is that no quaternary ammonium salt-modified fluorine-containing epoxy resin is added.
[0064] Prepare a 20 mg / L Cd-containing 2+ , Pb 2+ 、Zn 2+ 500 mL of simulated water samples were adjusted to pH 6 and placed on a program-controlled coagulation test stirrer. A flocculant containing modified L-arginine was added and stirred at a speed of 140 r / min for 2 min, then slowly stirred at a speed of 50 r / min for 15 min. After settling for 20 min, the clear liquid at 2 cm below the liquid surface was taken and the residual Cd was determined by atomic absorption spectrophotometer. 2+ , Pb 2+ 、Zn 2+ The test results are shown in Table 1.
[0065] Table 1: Cd 2+ , Pb 2+ 、Zn 2+ Concentration test.
[0066] project <![CDATA[Cd after treatment 2+ Concentration (mg / L)]]> <![CDATA[Pb after treatment 2+ Concentration (mg / L)]]> <![CDATA[Zn after treatment 2+ Concentration (mg / L)]]> Example 1 0.058 0.068 0.064 Example 2 0.064 0.072 0.052 Example 3 0.067 0.065 0.071 Example 4 0.075 0.058 0.057 Comparative Example 1 3.85 2.06 2.45 Comparative Example 2 2.73 1.65 2.07
[0067] As shown in Table 1, compared with Comparative Examples 1-2, Cd2+ , Pb 2+ 、Zn 2+ The concentration decreases and has a better flocculation effect.
[0068] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A flocculant containing modified L-arginine, It is characterized in that The invention comprises the following components by weight: 24-28 parts by weight of chitosan-modified L-arginine-modified polyurethane, 16-20 parts by weight of quaternary ammonium salt-modified fluorine-containing epoxy resin, 10-14 parts by weight of polyacrylamide, and 4-8 parts by weight of aluminum chloride; The preparation method of the chitosan-modified L-arginine-modified polyurethane is as follows: (1) Add chitosan to deionized water, stir to dissolve, add a mixed solution of thioglycolic acid and 1-ethyl-(3-dimethylaminopropyl)carbodiimide condensation agent, adjust the pH to 4-6, heat in a water bath, filter, wash and dry after the reaction is completed to obtain intermediate 1; (2) adding intermediate 1 to N,N-dimethylformamide solvent, stirring and dispersing, adding divinyl glycol and benzoin dimethyl ether photoinitiator, irradiating with 365 nm ultraviolet light at 25-40° C., centrifuging, washing and drying to obtain intermediate 2; (3) adding intermediate 2, L-arginine and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, stirring and mixing, reacting at 45-65°C for 2-4h, and after the reaction, vacuum distilling and drying to obtain chitosan-modified L-arginine chain extender; (4) Add fluoroketone diisocyanate and polyoxypropylene glycol to the reactor, then add dibutyltin dilaurate, introduce nitrogen protection, carry out prepolymerization at 85-90°C for 2.5-3h, then add chitosan-modified L-arginine chain extender to carry out chain extension reaction for 0.5-1.5h. After the reaction is completed, cool, wash and dry to obtain chitosan-modified L-arginine modified polyurethane; The preparation method of the quaternary ammonium salt modified fluorine-containing epoxy resin is: S1. Add 2-fluoro-phenylalanine and cyanuric acid epoxy resin to N,N-dimethylformamide solvent, react at 32-40°C for 1.2-2h, filter, wash and dry to obtain intermediate 3; S2. Add intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid catalyst to N,N-dimethylformamide solvent, introduce nitrogen protection, react at 80-100°C for 3.5-5.5h, and after the reaction is completed, cool, wash and dry to obtain intermediate 4; S3. Add intermediate 4 and bromoethanol to tetrahydrofuran solvent, stir and mix, react at 85-95 ° C for 6-8h, and after the reaction is completed, cool, wash and dry to obtain a quaternary ammonium salt-modified fluorinated epoxy resin; The preparation method of the flocculant containing modified L-arginine is: Chitosan-modified L-arginine-modified polyurethane, quaternary ammonium salt-modified fluorine-containing epoxy resin, polyacrylamide and aluminum chloride are added into a reactor, and stirred at a speed of 1200-1300 rpm for 5-10 minutes to obtain a flocculant containing modified L-arginine.
2. The flocculant containing modified L-arginine according to claim 1, It is characterized in that The heating temperature in (1) is 35-45°C and the heating time is 3.5-4h.
3. The flocculant containing modified L-arginine according to claim 1, It is characterized in that The ultraviolet light irradiation time in (2) is 2.5-3h.
4. The flocculant containing modified L-arginine according to claim 1, It is characterized in that The mass ratio of the intermediate 2, L-arginine and p-toluenesulfonic acid catalyst in (3) is 1:0.8-1.2:0.03-0.
05.
5. The flocculant containing modified L-arginine according to claim 1, It is characterized in that The mass ratio of fluoroquinone diisocyanate, polyoxypropylene glycol, dibutyltin dilaurate, and chitosan-modified L-arginine chain extender in (4) is 1:1.3-1.5:0.02-0.03:0.7-0.
9.
6. The flocculant containing modified L-arginine according to claim 1, It is characterized in that The mass ratio of 2-fluoro-phenylalanine to cyanuric acid epoxy resin in S1 is 1:1.3-1.
34.
7. The flocculant containing modified L-arginine according to claim 1, It is characterized in that The mass ratio of the intermediate 3, 3-hydroxy-N,N-diethylaniline and p-toluenesulfonic acid in S2 is 1:0.85-0.9:0.02-0.
05.
8. The flocculant containing modified L-arginine according to claim 1, It is characterized in that The mass ratio of the intermediate 4 to bromoethanol in S3 is 1:0.9-0.95.