Core-shell type hydrogen therapeutic agent as well as preparation method and application thereof
By wrapping a dense calcium carbonate shell on the surface of magnesium oxide-based particles and using the vapor deposition method to achieve controlled release of hydrogen, it solves the problem of clinical difficulty in maintaining sufficient concentration and duration of hydrogen at the disease site, significantly improving the therapeutic effect and Bioavailability.
Patent Information
- Application Number
- CN202410859076.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
AI Technical Summary
The low solubility and high diffusivity of hydrogen make it difficult to achieve targeted controlled release in clinical practice, resulting in poor therapeutic effects. It is difficult for existing technology to maintain sufficient hydrogen concentration and duration at the disease site.
The vapor deposition method is used to wrap a dense calcium carbonate shell on the surface of magnesium oxide-based particles. Through the joint action of calcium, magnesium and hydrogen, the controlled and sustained release of hydrogen is achieved, improving bioavailability and therapeutic effect.
It significantly improves the bioavailability of hydrogen, achieves long-term controlled release, enhances the therapeutic effect on diseased parts, and improves biocompatibility and efficacy through the synergistic effect of an appropriate amount of calcium and magnesium ions.
Smart Images

Figure CN118845828A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of biomedical materials, and in particular, relates to a core-shell hydrogen therapeutic agent and a preparation method and application thereof. Background Art
[0002] Physiologically active gases including nitric oxide (NO), carbon monoxide (CO), sulfur dioxide (SO2), hydrogen sulfide (H2S) and hydrogen (H2) have been developed as new therapies for antibacterial, antitumor and vascular regulation. The efficacy and biosafety of gas therapy depend on the concentration and residence time of the gas in the lesion site. If the concentration is insufficient, the therapeutic effect cannot be achieved, and excessive concentration of gas in the blood may cause systemic toxicity. Compared with other gases, safety is a prominent advantage in the application of H2. On the one hand, as an endogenous gas in the human body, H2 itself can be produced by colonic flora. On the other hand, the only product of H2 reaction is water, and no toxic byproducts remain. Unlike other components used in gas therapy such as NO and CO, local high concentrations of hydrogen will not interact with red blood cells and therefore have no blood toxicity. In diving medicine, there is already a hydrogen-oxygen mixed gas supply method, which is safe and has no adverse reactions to the human body. Many countries have included hydrogen in the list of food additives. Clinically, through methods such as inhaling hydrogen, injecting hydrogen-rich saline and drinking hydrogen-containing water, it has been confirmed that hydrogen has antioxidant, anti-tumor, anti-apoptosis and anti-inflammatory functions, as well as beneficial effects in the treatment of diseases such as cancer, stroke, diabetes, arthritis, dermatitis, etc.
[0003] As a therapeutic drug, there is a gap in the pharmacokinetic research of hydrogen. The low solubility of hydrogen makes it difficult to effectively accumulate at the target location, and continuous administration is required. The high permeability and easy diffusion allow hydrogen to pass through the blood-brain barrier to reach sites that other drugs cannot treat, but this penetration is not targeted and the therapeutic effect is limited. Ammonia borane, palladium-based, iron-based and other materials have been shown to release hydrogen under physiological conditions, but the hydrogen production is low, so it is usually necessary to combine other treatment methods (such as photothermal therapy, photodynamic therapy, chemotherapy) for disease treatment. Magnesium-based active metals react with water to produce a large amount of hydrogen. At the same time, magnesium is an essential constant element for the human body. Therefore, metallic magnesium has good biocompatibility, and magnesium-based hydrogen storage materials are the most favorable hydrogen therapeutic agents for clinical transformation.
[0004] The prior patent CN202311463600.7 modified the surface of magnesium bulk metal with nano-calcium carbonate particles to improve the tumor microenvironment, but the modification adopted a heat curing method. First, this method is not suitable for uniform surface modification of small-sized particles; second, the surface is modified with nano-calcium carbonate particles, and the coating has a non-dense structure due to the influence of the gaps between the particles; third, the CaCO3 coating prepared by the thermosetting method is easy to fall off, and the purpose of controlled hydrogen release cannot be achieved.
[0005] Patent 201510838912.0 discloses a composite modified coating containing carbon nanotubes on the surface of magnesium or magnesium alloy and its preparation method, which uses pure magnesium or magnesium alloy as the base material, and uses the micro-arc oxidation method to evenly cover a layer of magnesium phosphate / magnesium oxide transition layer with a microporous structure on its surface, and then uses the electrophoretic deposition method to evenly cover a layer of carbon nanotube-hydroxyapatite coating on it. On the surface of the pure magnesium or magnesium alloy with a micro-arc oxidation transition layer with a microporous structure, a carbon nanotube composite powder with hydroxyapatite wrapped on the surface is deposited by a low-temperature electrodeposition process, and some carbon nanotubes can enter the micropores of the micro-arc oxidation transition layer, further enhancing the bonding strength of the composite coating and improving the wear resistance and toughness of the coating. However, the transition layer used in this method is a microporous magnesium phosphate / magnesium oxide transition layer that is not dense, and the preparation method of the hydroxyapatite layer is a low-temperature electrodeposition process. This method is only suitable for single-layer surface coating of block or sheet metals with relatively flat surfaces and large surface areas, and is not suitable for uniform modification of the overall surface of small-sized particles, and the application scenarios are limited.
[0006] The low solubility and high diffusivity of hydrogen limit its clinical application, and the targeted and controlled release of hydrogen is crucial for its application. Based on this, the present invention adopts magnesium-based materials and performs surface modification by vapor deposition to achieve the controlled and continuous release of hydrogen, and improves the therapeutic effect on the diseased site through the joint action of calcium, magnesium and hydrogen, thereby achieving synergistic treatment. Summary of the invention
[0007] The purpose of the present invention is to provide a core-shell hydrogen therapeutic agent and its preparation method and application, in view of the problems of insufficient hydrogen concentration at the target site of the disease in the existing traditional hydrogen therapy, poor efficacy of hydrogen treatment alone, and too fast and unsustainable early hydrogen burst release of magnesium-based materials in the body. The present invention adopts a vapor deposition method to wrap a dense calcium carbonate shell layer on the surface of the oxidized magnesium-based particles, which can greatly improve the stability of its aqueous solution, effectively regulate the hydrogen release kinetics, inhibit the rapid burst release and escape of hydrogen, achieve controllable long-term and sustained hydrogen release, and significantly improve the bioavailability in the body. At the same time, the appropriate amount of calcium and magnesium ions and hydrogen produced by the controllable degradation of the therapeutic agent can achieve synergistic biological effects, increase synergy and reduce toxicity, and show excellent biocompatibility and biological activity to normal cells and tissues.
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] A method for preparing a core-shell hydrogen therapeutic agent comprises the following steps:
[0010] (1) oxidizing the surface of the magnesium-based particles to obtain magnesium-based particles coated with magnesium oxide;
[0011] (2) dispersing calcium salt in an organic solvent to obtain a reaction system A; dispersing magnesium-based particles coated with magnesium oxide in an organic solvent to obtain a reaction system B; mixing the reaction system A and the reaction system B to obtain a mixture C;
[0012] (3) placing carbonate powder in container A and mixture C in container B; placing container A and container B adjacent to each other and heating them under vacuum, and after a certain temperature and a period of reaction, centrifuging the material in container B and collecting the precipitate; wherein the tops of container A and container B are open or have air holes;
[0013] (4) Washing the precipitate of step (3), removing the supernatant by centrifugation, and drying to obtain the core-shell hydrogen therapeutic agent.
[0014] The magnesium-based particles include magnesium hydrogen particles (MgH x , x=2-6), one or more of magnesium powder (Mg), magnesium-based organic framework particles, and magnesium alloy composite particles.
[0015] The magnesium-based organic framework structure particles include one or more of Mg-MOF, Mg-COF, Mg-Fe, and Mg-Zn.
[0016] The diameter of the magnesium-based particles is 0.1-100 μm.
[0017] The magnesium alloy composite particles include Mg-Fe and Mg-Zn.
[0018] In step (1), the oxidation method adopts DC arc plasma evaporation method, and air is introduced into the reaction chamber during cooling until the reaction chamber returns to atmospheric pressure.
[0019] In step (1), the surface oxidation step is: 0.05-0.08atm of air is filled into the reaction chamber every 30-60 minutes until the reaction chamber reaches atmospheric pressure.
[0020] In step (2), the calcium salt includes calcium nitrate and / or calcium chloride;
[0021] In step (2), in the mixture C, the molar ratio of the magnesium-based particles coated with magnesium oxide to the calcium ions in the calcium salt is 1:0.2-2.
[0022] In step (2), the organic solvent includes at least one of ethanol, n-propanol, n-butanol / isobutanol, ethylene glycol, glycerol, and tetrahydrofuran.
[0023] In step (3), the vacuum heating container is a vacuum drying oven.
[0024] In step (3), the carbonate includes one or more of ammonium bicarbonate NH4HCO3, NaHCO3, and CaCO3. The carbonate decomposes under heat to produce CO2, forming a calcium carbonate shell.
[0025] Preferably, the carbonate is NH4HCO3.
[0026] CO3 in the carbonate in step (3) 2- With the calcium salt in step (2) Ca 2+ The molar ratio is 50:1-400:1.
[0027] Step (3) specifically comprises placing the mixture C and the carbonate adjacent to each other in a vacuum drying oven, including standing and / or placing the mixture in the oven without an electric shaker; the heating temperature is 37-45° C., and the reaction time is 12-120 h.
[0028] If the heating temperature is too high, the carbonate will decompose rapidly, and CO2 and Ca will spontaneously nucleate to form CaCO3 particles; if the heating temperature is too low, the carbonate will not decompose easily and will not produce enough CO2 reaction gas.
[0029] The hydrogen therapeutic agent is spherical.
[0030] The use of the core-shell hydrogen therapeutic agent in the preparation of anti-tumor, anti-inflammatory and antibacterial drugs also falls within the protection scope of the present invention.
[0031] This includes the use in the preparation of drugs for treating local tissue inflammation, bacterial infection, tumors and other diseases. More preferably, it can be used in medical applications such as various types of arthritis, gastroenteritis, wound repair, and prevention of recurrence after bone tumor resection.
[0032] The synthesis process of the core-shell hydrogen therapeutic agent is simple, easy, efficient and reproducible, and can be used for large-scale production.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1. The present invention wraps a magnesium oxide-calcium carbonate composite shell layer outside the magnesium-based material to construct a core-shell hydrogen therapeutic agent. The wrapping of the magnesium oxide-calcium carbonate composite shell layer slows down the excessive hydrogen release of the magnesium-based particles in the human body, and is easy to respond to the microenvironment of the disease site, thereby achieving local slow controlled release of hydrogen. The long-term controlled release of hydrogen allows the therapeutic agent to maintain an effective therapeutic concentration of hydrogen at the treatment site for a longer period of time, thereby improving the bioavailability of hydrogen and the hydrogen therapeutic agent, thereby effectively treating the disease.
[0035] 2. The method used is the oxidation composite vapor deposition method, which has simple steps and is easy to mass produce. Using it to wrap magnesium-based particles helps the constructed hydrogen sustained-release system to be transformed into clinical applications more quickly. The unique advantages of this core-shell hydrogen therapeutic agent are: ① The dense magnesium oxide-calcium carbonate composite shell layer can reduce the reaction between magnesium-based particles and water, reduce self-degradation, and facilitate long-term storage; ② It can utilize endogenous stimulation of the disease site (low pH; high Cl - , HCO3 - anion concentration), generating therapeutic H2 gas in situ to achieve the therapeutic purpose.
[0036] 3. The appropriate amount of calcium, magnesium ions and hydrogen produced by the controlled degradation of the therapeutic agent can also achieve synergistic biological effects, improve the efficacy of tumors, bacteria and inflammatory diseases, while showing excellent biocompatibility with normal cells and tissues, and can also synergistically induce biological activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0038] Figure 1 Surface element analysis of MgH2-MgO after oxidation treatment synthesized in Example 1.
[0039] Figure 2 This is the transmission electron microscopy result of the core-shell hydrogen therapeutic agent MgH2-MgO in Example 1.
[0040] Figure 3 Transmission electron microscopy results of the hydrogen therapeutic agent Mg-Fe-MgO@CaCO3 synthesized in Example 4.
[0041] Figure 4 Transmission electron microscopy results of the hydrogen therapeutic agent MgH2-MgO@CaCO3 synthesized in Example 3.
[0042] Figure 5 Particle size results of comparative example 3Mg-Fe@CaCO3.
[0043] Figure 6 The hydrogen release test results of the hydrogen therapeutic agents MgH2-MgO@CaCO3 and MgH2@CaCO3 synthesized in Example 3 and Comparative Example 1 in PBS solution (pH 6.5); wherein A is MgH2-MgO@CaCO3 of Example 3; and B is MgH2@CaCO3 of Comparative Example 1.
[0044] Figure 7 The tumor cell killing test results of the hydrogen therapeutic agents MgH2-MgO@CaCO3 and MgH2@CaCO3 synthesized in Example 3 and Comparative Example 1.
[0045] Figure 8 Tumor treatment results of the hydrogen therapeutic agent MgH2-MgO@CaCO3 synthesized in Example 3.
[0046] Fig. 9 Example 3. Safety results of the hydrogen therapeutic agent MgH2-MgO@CaCO3 for tumor treatment.
[0047] Fig.10 Example 3 The therapeutic effect of the synthesized therapeutic agent MgH2-MgO@CaCO3 on osteoarthritis in SD rats. DETAILED DESCRIPTION
[0048] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0049] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0050] Example 1 Synthesis of core-shell hydrogen therapeutic agent MgH2-MgO
[0051] Surface oxidation treatment of magnesium-based particles: magnesium powder (purity 99.995%, particle size 100-200 mesh) is pressed into cylindrical anode material under a pressure of 15 MPa, and then evaporated by DC arc plasma (vacuum degree less than 5*10 -2 Pa, the reaction gas is hydrogen, the arc is started at a current of 30A, and the current is adjusted to 120A after stabilization), and then 0.05atm of air is slowly introduced into the reaction chamber every 30min (for a total of 6h) until the reaction chamber reaches atmospheric pressure; an oxide film (with a thickness of 20nm) is produced on the surface of MgH2 to obtain MgH2-MgO (particle size of 200-700nm) with a core-shell structure; and the internal MgH2 is protected from oxidation and water corrosion.
[0052] like Figure 1 Surface element analysis of the core-shell MgH2-MgO synthesized in Example 1.
[0053] Figure 2 This is the transmission electron microscopy result of the core-shell hydrogen therapeutic agent MgH2-MgO in Example 1.
[0054] Example 2 Synthesis of Core-Shell Hydrogen Therapeutic Agent Mg-Fe-MgO
[0055] Surface oxidation treatment of magnesium-based particles: Mix magnesium powder Mg (purity 99.995%, particle size 100-200 mesh) and transition metal Fe at a mass ratio of 95:5. In a hydraulic tablet press, maintain a pressure of 20 MPa for 2 minutes to obtain a small cylinder with H = 2 cm and Ф = 2 cm as the anode material. After DC arc plasma evaporation (vacuum degree less than 5*10 -2 Pa, the reaction gas is a mixture of 0.07MPa argon and 0.01MPa hydrogen, the arc is started with a current of 30A, and the current is adjusted to 120A after stabilization). After obtaining Mg-Fe particles (particle size is about 200), 0.05atm air is slowly introduced into the reaction chamber every 60min (4 times in total) until the reaction chamber reaches atmospheric pressure to produce an oxide film (20nm) on the surface of Mg-Fe, thereby producing a core-shell structure (Mg-Fe-MgO) to protect the internal Mg-Fe from oxidation and water corrosion.
[0056] Example 3: Synthesis of core-shell hydrogen therapeutic agent MgH2-MgO@CaCO3
[0057] Synthesis of MgH2-MgO@CaCO3: Weigh 50mg CaCl2 and 25mg MgH2-MgO with a diameter of 200-300nm prepared in Example 1, disperse them in 100ml ethanol and place them in a 200ml beaker. Wrap the beaker mouth with tin foil and punch holes. Weigh 10g ammonium bicarbonate, place it in a dish, place it adjacent to the beaker in a vacuum oven, let it stand for 24h under vacuum at 40℃, collect the liquid in the beaker, centrifuge it at 25℃, 1000rpm, 10min, and discard the supernatant. The precipitate is dispersed in ethanol again, centrifuged at 25℃, 1000rpm, 10min, discard the supernatant, and after repeated washing, place the resulting precipitate in a vacuum oven and vacuum dry it at 40℃. The resulting precipitate is MgH2-MgO@CaCO3.
[0058] Characterization:
[0059] 1) Observation by transmission electron microscope and determination by particle size analyzer. The specific methods are as follows:
[0060] The MgH2-MgO@CaCO3 prepared in the above steps was ultrasonically dispersed in anhydrous ethanol (the concentration of the therapeutic agent was 1 mg / mL), 10 μL of the solution was taken and dropped onto a carbon-coated copper mesh (300 mesh, Zhongjing Ke Instrument), and naturally air-dried at room temperature. Under a voltage of 200KV, the morphology, particle size and element distribution of the nanoparticles were observed by transmission electron microscopy. The results of transmission electron microscopy showed that the main elements on the surface of the oxidized magnesium-based particles were Mg and O, and the core-shell hydrogen therapeutic agent was spherical in shape, with magnesium-based particles inside and a magnesium oxide-calcium carbonate composite thin layer wrapped on the surface. The thickness of CaCO3 is about 30-50nm ( Figure 4 ).
[0061] 2) Inductively coupled plasma emission spectrometer (ICP) detection of MgH2-MgO@CaCO3 related element content analysis: Weigh 2 mg of MgH2-MgO@CaCO3 obtained in Example 3, dissolve it in 2% dilute nitric acid, and let it stand for 24 hours until no solid remains in the solution. Through ICP measurement, it can be known that the content ratio of Ca element and Mg element in MgH2-MgO@CaCO3 in Example 3 is about 1:20.
[0062] Example 4: Synthesis of core-shell hydrogen therapeutic agent Mg-Fe-MgO@CaCO3
[0063] Synthesis of Mg-Fe-MgO@CaCO3:
[0064] Weigh 50 mg of CaCl2 and add it to 50 ml of ethanol, and disperse by ultrasonic to obtain reaction system A;
[0065] Weigh 20 mg of Mg-Fe-MgO prepared in Example 2, add it into 50 ml of ethanol, and disperse it by ultrasonic to obtain reaction system B;
[0066] Reaction system A and reaction system B are mixed to obtain a uniform and stable reaction system C. Reaction system C is placed in a 200ml beaker, and the mouth of the beaker is wrapped and pierced. Weigh 10g of ammonium bicarbonate, place it in a dish, and place it in a vacuum oven adjacent to the beaker. Shake it on a shaker at a speed of 100rpm / min under 40℃ vacuum conditions for 24h, collect the liquid in the beaker, centrifuge it at 25℃, 1000rpm, 10min, and discard the supernatant. The precipitate is dispersed in ethanol again, centrifuged at 25℃, 1000rpm, 10min, and the supernatant is discarded. After repeated washing, the obtained precipitate is placed in a vacuum oven and vacuum dried at 40℃. The obtained precipitate is Mg-Fe-MgO@CaCO3.
[0067] According to transmission electron microscopy observations ( Figure 3 ) and a particle size analyzer (the testing method is the same as in Example 2), the thickness of CaCO3 is about 20-50nm.
[0068] Comparative Example 1
[0069] The only difference between this comparative example and Example 3 is that MgH2-MgO is replaced by MgH2 with a diameter of 200 nm.
[0070] Synthesis of MgH2@CaCO3: Weigh 50mg CaCl2 and 25mg MgH2 with a diameter of 200nm, disperse them in 100ml ethanol and place them in a 200ml beaker. Wrap the mouth of the beaker with tin foil and punch holes. Weigh 10g ammonium bicarbonate, place it in a dish, place it next to the beaker in a vacuum oven, let it stand for 24h under vacuum at 40℃, collect the liquid in the beaker, centrifuge it at 25℃, 1000rpm, 10min, and discard the supernatant. The precipitate is dispersed in ethanol again, centrifuged at 25℃, 1000rpm, 10min, discard the supernatant, and repeat the washing once. Place the resulting precipitate in a vacuum oven and dry it in vacuum at 40℃. The resulting precipitate is MgH2@CaCO3.
[0071] Comparative Example 2
[0072] The difference between this comparative example and Example 3 is only that no CaCl2 is added.
[0073] Weigh 25 mg of MgH2-MgO prepared in Example 1, disperse it in 100 ml of ethanol and place it in a 200 ml beaker. Wrap the mouth of the beaker with tin foil and punch holes. Weigh 10 g of ammonium bicarbonate, place it in a dish, place it in a vacuum oven adjacent to the beaker, let it stand for 24 hours under vacuum at 40°C, collect the liquid in the beaker, centrifuge it at 25°C, 1000 rpm, 10 min, and discard the supernatant. The precipitate is dispersed in ethanol again, centrifuged at 25°C, 1000 rpm, 10 min, discard the supernatant, and repeat the washing once. Place the resulting precipitate in a vacuum oven and vacuum dry it at 40°C. The resulting precipitate does not form a CaCO3 shell.
[0074] Comparative Example 3
[0075] The only difference between this comparative example and Example 4 is that Mg—Fe—MgO is replaced by Mg—Fe with a diameter of 200 nm.
[0076] Synthesis of Mg-Fe@CaCO3: Weigh 50mg CaCl2 and add it to 50ml ethanol, ultrasonically disperse it to obtain reaction system A, weigh 20mg (Mg-Fe) with a diameter of 200nm and add it to 50ml ethanol, ultrasonically disperse it to obtain reaction system B, mix reaction system A with reaction system B to obtain a uniform and stable reaction system C, place reaction system C in a 200ml beaker, wrap the mouth of the beaker and punch holes. Weigh 10g ammonium bicarbonate, place it in a dish, place it adjacent to the beaker in a vacuum oven, shake it on a shaker at a speed of 100rpm / min under 40℃ vacuum conditions for 24h, collect the liquid in the beaker, centrifuge it at 25℃, 1000rpm, 10min, and discard the supernatant. The precipitate is dispersed in ethanol again, centrifuged at 25℃, 1000rpm, 10min, discard the supernatant, and repeat the washing once. The resulting precipitate is placed in a vacuum oven and vacuum dried at 40℃. The resulting precipitate is Mg-Fe@CaCO3. According to the observation under transmission electron microscope and the measurement by particle size analyzer, Mg-Fe@CaCO3 is spherical and the particle size is about 288nm.
[0077] Comparative Example 4
[0078] The difference between this comparative example and Example 3 is that: the CaCO3 coating is prepared by a thermosetting method, 20 mg of calcium carbonate powder (Aladdin) is added to 15% (mass concentration) of organic polysilazane (OPSZ) in butyl acetate, and ultrasonically dispersed to form a dispersion (ultrasonic conditions: 35 KHz, 10 min), 100 mg of MgH2-MgO prepared in Example 1 is added to the dispersion, and further ultrasonically dispersed (ultrasonic conditions: 35 KHz, 10 min), and then heated and cured (heating temperature: 37°C; time 24 h). The resulting precipitate is severely agglomerated and cannot form monodisperse MgH2-MgO@CaCO3 particles.
[0079] Comparative Example 5
[0080] The difference between this comparative example and Example 3 is that ammonium bicarbonate NH4HCO3 is replaced by hydroxyapatite (HAP).
[0081] Results: Hydroxyapatite (HAP) cannot produce CO2 under vacuum conditions and cannot form a calcium carbonate shell.
[0082] Performance Test Example 1
[0083] Image J was used to measure the particle size of the hydrogen therapeutic agent: The transmission electron microscope photos were measured using Image J software, and the average value was taken after six repetitions. The diameters of the Mg-Fe-MgO prepared in Example 4 and the Mg-Fe@CaCO3 prepared in Example 2 were measured before and after encapsulation. The results are shown in Table 1. The average particle size of Example 4 (Mg-Fe-MgO) was approximately 350±14.5 nm, and the particle size of Example 2 (Mg-Fe-MgO@CaCO3) was approximately 439.7±21.4 nm.
[0084] Table 1 Example 2 (Mg-Fe-MgO) particle size measurement results
[0085] serial number Measurement results (nm) 1 364.6 2 346.8 3 356.7 4 344.3 5 349.8 6 338.5 Average particle size 350.1±14.5
[0086] Table 2 Mg-Fe-MgO@CaCO3 particle size measurement results
[0087] Data No. Measurement results (nm) 1 433.1 2 452.9 3 418.3 4 447.2 5 450.2 6 436.4 Average particle size 439.7±21.4
[0088] Performance Test Example 2 Characterization of Hydrogen Release of Core-Shell Therapeutic Agents
[0089] The specific steps are as follows:
[0090] Weigh 3 mg of MgH2-MgO@CaCO3 of Example 3 and MgH2@CaCO3 of Comparative Example 1, respectively, and place them in a 12-well plate; add 3 mL of PBS to the well to be tested to make a 1 mg / ml solution. Place the hydrogen measuring pen in the solution for measurement. Measure at 1 min, 5 min, 10 min, 30 min, 1 h, 2 h, 4 h, 6 h, 8 h, 10 h, 24 h, 48 h, and 72 h after adding PBS with a pH of 6.5. The results are shown in the figure. Figure 6 The MgH2@CaCO3 obtained in Comparative Example 1 and the MgH2@CaCO3 obtained in Example 3 are shown. 2- Comparison of in vitro hydrogen release of MgO@CaCO3, Figure 6 A is MgH2-MgO@CaCO3, Figure 6 B is MgH2@CaCO3, and it can be seen that the core-shell MgH2-MgO@CaCO3 can obviously achieve the purpose of sustained release under acidic conditions. 2- MgO@CaCO3 can maintain a relatively high hydrogen release concentration in the first 24 hours, while MgH2@CaCO3 shows a gradually decreasing trend.
[0091] Performance Test Example 3 Tumor Killing Experiment of Core-Shell Therapeutic Agent
[0092] The specific steps are as follows:
[0093] B16 melanoma cell killing experiment: B16 cells were seeded in a 96-well cell culture plate at a density of 5000 cells / well. After the cells adhered to the wall, different concentrations of MgH2 (62.5 and 250 μg / mL) and MgH2-MgO@CaCO3 (62.5 and 250 μg / mL) solutions of Example 3 were added, and the cell viability was detected using the CCK8 kit (Japan Tongren) after incubation for 24 hours. The test results are shown in Figure 2. Figure 7 As shown, compared with MgH2 particles, the MgH2 particles of Example 3 2- -MgO@CaCO3 can kill B16 melanoma cells more significantly and effectively, and has the potential to treat melanoma.
[0094] Performance Test Example 4 Tumor Treatment and Efficacy Monitoring of Core-Shell Therapeutic Agents
[0095] The specific steps are as follows: 125 μL (5 mg / mL) of MgH2-MgO@CaCO3 of Example 3 or the control group (PBS) was injected into the tumor-bearing mice through the tail vein. The treatment lasted for 14 days, with medication every 3 days, and the volume and weight of the mice were weighed every 2 days. The tumor volume and weight of different mice at different time points after treatment were dynamically monitored. Compared with the PBS group, the tumor volume growth of mice in the MgH2-MgO@CaCO3 treatment group was significantly slowed down ( Figure 8 ), there was no significant difference in the body weight of mice in each group ( Fig. 9 ).
[0096] Performance Test Example 5 Therapeutic Effect of Core-Shell Therapeutic Agent on Osteoarthritis in SD Rats
[0097] The specific steps are as follows: SD rats were divided into an experimental group and a control group, with 6 rats in each group; the anterior cruciate ligament (ACL) was cut off in the control group and the experimental group to prepare the rat KOA model. Four weeks after surgery, the rats in the experimental group were injected with MgH2-MgO@CaCO3 saline solution (5 mg / mL) into the KOA joint, and the rats in the control group were injected with the same dose of saline. Each group of rats was injected once every 10 days, with 100 μL injected each time. After 40 days of treatment, the rats were killed and the knee joints of the rats were taken. The Mankin's score system and the OARSI knee soft tissue inflammation scoring system were used to quantitatively evaluate the degree of articular cartilage damage and the degree of inflammatory response in the synovium between different groups. The smoothness, color, and degree of cartilage wear of the knee cartilage surface were statistically analyzed. The results showed that the Mankin score and OARSI score of the experimental group were significantly lower than those of the control group, indicating that the knee cartilage damage in the experimental group was better than that in the control group. ( Fig.10 )The results showed that MgH2-MgO@CaCO3 can treat osteoarthritis, and its degradation products calcium, magnesium and hydrogen can synergistically inhibit cartilage destruction and relieve inflammation.
[0098] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A method for preparing a core-shell hydrogen therapeutic agent, characterized in that: The steps include: (1) oxidizing the surface of the magnesium-based particles to obtain magnesium-based particles coated with magnesium oxide; (2) dispersing calcium salt in an organic solvent to obtain a reaction system A; dispersing magnesium-based particles coated with magnesium oxide in an organic solvent to obtain a reaction system B; mixing the reaction system A and the reaction system B to obtain a mixture C; (3) placing carbonate powder in container A and mixture C in container B; placing container A and container B adjacent to each other and heating them under vacuum, and after a certain temperature and a period of reaction, centrifuging the material in container B and collecting the precipitate; wherein the tops of container A and container B are open or have air holes; (4) Washing the precipitate of step (3), removing the supernatant by centrifugation, and drying to obtain the core-shell hydrogen therapeutic agent.
2. The preparation method according to claim 1, characterized in that: In step (1), the surface oxidation step is: 0.05-0.08atm of air is filled into the reaction chamber every 30-60 minutes until the reaction chamber reaches atmospheric pressure.
3. The preparation method according to claim 1, characterized in that: In step (1), the magnesium-based particles include one or more of magnesium hydrogen particles, magnesium powder, magnesium-based organic framework particles, and magnesium alloy composite particles.
4. The preparation method according to claim 1, characterized in that: In step (2), the calcium salt includes calcium nitrate and / or calcium chloride.
5. The preparation method according to claim 1, characterized in that: In step (2), in the mixture C, the molar ratio of magnesium ions in the magnesium-based particles coated with magnesium oxide to calcium ions in the calcium salt is 1:0.2-2.
6. The preparation method according to claim 1, characterized in that: In step (3), the vacuum heating container is a vacuum drying oven.
7. The preparation method according to claim 1, characterized in that: In step (3), the carbonate includes one or more of NH4HCO3, NaHCO3, and CaCO3.
8. The preparation method according to claim 1, characterized in that: CO3 in the carbonate in step (3) 2- With the calcium salt in step (2) Ca 2+ The molar ratio is 50:1-400:
1.
9. A core-shell hydrogen therapeutic agent prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the core-shell hydrogen therapeutic agent according to claim 9 in the preparation of anti-tumor, anti-inflammatory and antibacterial drugs.