Mineral processing technology for recovering rare earth, fluorite and barite from rare earth tailings
Through the multi-step mixed flotation process of rare earth and fluorite, strong magnetic separation and shaking table gravity separation, the problem of neglecting the recovery of fluorite and barite in the existing technology is solved, and the efficient recovery of rare earth, fluorite and barite is achieved. and separation, improving resource utilization.
Patent Information
- Application Number
- CN202411191802.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-10-29
AI Technical Summary
The existing rare earth mining process ignores the secondary development and recovery value of fluorite and barite, resulting in a waste of resources.
A multi-step rare earth and fluorite mixed flotation process is adopted, including grinding fineness test, sodium carbonate and water glass dosage test, inhibitor and collector dosage test, open circuit test and closed circuit test, combined with strong magnetic separation and shaking table Gravity separation to achieve efficient recovery of rare earths, fluorite and barite.
It achieves high-efficiency recovery and separation of rare earths and fluorite, and efficient recovery of barite, improves resource utilization and meets the quality requirements of industrial standards.
Smart Images

Figure CN118847351A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of mineral processing, in particular to a mineral processing process for recovering rare earth, fluorite and barite from rare earth tailings. Background Art
[0002] Fluorite for metallurgical industry is also called metallurgical grade fluorite. It is mainly used as a solvent for metallurgical slag to reduce the melting point of the slag and improve the fluidity of the metallurgical slag. Metallurgical grade fluorite is generally a fluorite concentrate product produced from fluorite ore by hand selection, jigging, heavy medium or flotation. Barite is an important non-metallic mineral with high specific gravity, low hardness, non-toxicity, non-magneticity, stable chemical properties, insoluble in water and acid, and able to absorb X-rays and gamma rays. It is often used in industries such as petroleum, chemical industry, paint and filler. Due to its high density, it can also be used as a weighting agent for oil and natural gas drilling mud.
[0003] In the existing rare earth mining process, due to the limitations of the existing mineral processing technology, fluorite and barite associated with rare earth ores are often treated as solid wastes, and their value for secondary development and recycling is ignored.
[0004] Therefore, it is necessary to design a mineral processing process for recovering rare earths, fluorite and barite from rare earth tailings, and to achieve efficient and comprehensive utilization of barite and fluorite through the combination of multiple processes. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a beneficiation process for recovering rare earth, fluorite and barite from rare earth tailings, thereby achieving efficient comprehensive utilization of fluorite and barite in rare earth tailings.
[0006] In order to achieve the above object, the present invention provides a beneficiation process for recovering rare earth, fluorite and barite from rare earth tailings, comprising the following steps:
[0007] S1, rare earth and fluorite mixed flotation grinding fineness test:
[0008] The grinding concentration is 62.5%. Sodium carbonate 2000g / t is used for stirring for 3min, water glass 2000g / t is used for stirring for 3min, inhibitor TJ-1 200g / t is used for stirring for 3min, collector LT-1 600g / t is used for stirring for 2min, and then roughing for 5min is performed to obtain concentrate and tailings. It is confirmed that the best rare earth and fluorite mixed flotation grinding fineness is -200 mesh accounting for 80%;
[0009] S2, Sodium carbonate dosage test for roughing of rare earth and fluorite mixed flotation:
[0010] The grinding concentration is 62.5%, the grinding fineness is -200 mesh accounting for 80%, and 2000g / t of water glass is used for stirring for 3min, the inhibitor TJ-1 200g / t is used for stirring for 3min, and the collector LT-1 600g / t is used for stirring for 2min and roughing for 5min to obtain the concentrate and tailings, and it is confirmed that the optimal sodium carbonate dosage for the roughing of rare earth and fluorite mixed flotation is 1500g / t;
[0011] S3, water glass dosage test for roughing of rare earth and fluorite mixed flotation:
[0012] The S2 method was adopted, with water glass set as a variable and sodium carbonate set at 1500 g / t, to obtain concentrate and tailings, and it was confirmed that the optimal water glass dosage for the roughing of rare earth and fluorite mixed flotation was 2000 g / t;
[0013] S4, test on the dosage of barite inhibitor in the roughing of rare earth and fluorite mixed flotation:
[0014] The S3 method was adopted, the inhibitor TJ-1 was set as a variable, the water glass was set to 2000g / t, the concentrate and tailings were obtained, and the optimal dosage of the barite inhibitor TJ-1 for the roughing of rare earth and fluorite mixed flotation was confirmed to be 200g / t;
[0015] S5, rare earth and fluorite mixed flotation roughing collector dosage test:
[0016] The S4 method was used to set the collector LT-1 as a variable and the inhibitor TJ-1 as 200 g / t to obtain concentrate and tailings, and it was confirmed that the optimal dosage of the collector LT-1 for the roughing of rare earth and fluorite mixed flotation was 800 g / t.
[0017] S6, open circuit test of rare earth and fluorite mixed flotation:
[0018] S6-1, grinding concentration is 62.5%, grinding fineness is -200 mesh accounting for 80%, sodium carbonate 1500g / t is used for stirring for 3min, water glass 2000g / t is used for stirring for 3min, inhibitor TJ-1 200g / t is used for stirring for 3min, collector LT-1800g / t is used for stirring for 2min, and then roughing for 5min to obtain mixed rough concentrate and roughing tailings;
[0019] S6-2, the mixed coarse concentrate obtained in S6-1 is subjected to concentration one, and after stirring with 800 g / t of water glass for 3 minutes, a concentration two and a medium ore 4 are obtained; after stirring with 400 g / t of water glass for 3 minutes, a concentration three and a medium ore 3 are obtained; after stirring with 200 g / t of water glass for 3 minutes, a concentration four and a medium ore 2 are obtained; after concentrating the concentration four again, a concentrate and a medium ore 1 are obtained;
[0020] S6-3, the rough tailings obtained in S6-1 were scavenged by stirring with 800 g / t of sodium carbonate for 3 min, 1000 g / t of water glass for 3 min, 100 g / t of inhibitor TJ-1 for 3 min, 400 g / t of collector LT-1 for 2 min, and then scavenged for 4 min to obtain the middling ore 5 and tailings;
[0021] S7, Closed-circuit test of rare earth and fluorite mixed flotation:
[0022] S7-1, grinding concentration is 62.5%, grinding fineness is -200 mesh accounting for 80%, sodium carbonate 1500g / t is used for stirring for 3min, water glass 2000g / t is used for stirring for 3min, inhibitor TJ-1 200g / t is used for stirring for 3min, collector LT-1600g / t is used for stirring for 2min and then roughing for 5min;
[0023] S7-2, after roughing S7-1, select the first concentrate, stir with 800g / t of water glass for 3min to obtain select the second concentrate and the middle ore five; stir with 400g / t of water glass for 3min to obtain select the third concentrate and the middle ore four; stir with 200g / t of water glass for 3min to obtain select the fourth concentrate and the middle ore three; stir with 100g / t of water glass for 3min to obtain select the fifth concentrate and the middle ore two; select the fifth concentrate again to obtain the concentrate and the middle ore one;
[0024] S7-3, after roughing S7-1, stir with 800 g / t of sodium carbonate for 3 min, stir with 1000 g / t of water glass for 3 min, stir with 100 g / t of inhibitor TJ-1 for 3 min, stir with 300 g / t of collector LT-1 for 2 min, and then scavenge for 4 min to obtain the middle ore No. 6 and tailings; S7-4, mix the middle ore No. 5 and the middle ore No. 6 obtained in S7-2 and S7-3 and enter the step of S7-1 again;
[0025] S7-5, returning the medium ore No. 4 in S7-2 to the step of selecting No. 1 in S7-2;
[0026] S7-6, returning the medium ore 3 in S7-2 to the step of selecting the second in S7-2;
[0027] S7-7, returning the medium ore 2 in S7-2 to the step of fine selection 3 in S7-2;
[0028] S7-8, returning the medium ore 1 in S7-2 to the step of selecting 4 in S7-2;
[0029] S8, Mixed flotation concentrate rare earth and fluorite strong magnetic separation test:
[0030] The mixed flotation concentrate is subjected to a strong magnetic roughing separation with a magnetic field strength of 1.3T to obtain magnetic and non-magnetic materials, the non-magnetic materials are subjected to a strong magnetic sweeping separation with a magnetic field strength of 1.3T to obtain strong magnetic sweeping separation first intermediate ore and strong magnetic sweeping separation first tailings, and the strong magnetic sweeping separation tailings are subjected to a strong magnetic sweeping separation second with a magnetic field strength of 1.3T to obtain strong magnetic sweeping separation second intermediate ore and strong magnetic sweeping separation second tailings;
[0031] S9, rare earth and fluorite mixed flotation tailings gravity separation test:
[0032] After the mixed flotation tailings are roughly separated by shaking table gravity separation, tailings are obtained by shaking table gravity separation concentration 1, and then concentrate and tailings are obtained by bed gravity separation concentration 2.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] After a closed-circuit test of rare earth and fluorite mixed flotation with one roughing, five fines and one sweeping, a mixed concentrate with an operating yield of 5.71%, a TREO grade of 5.92%, a CaF2 grade of 91.24%, a TREO operating recovery rate of 59.32%, and a CaF2 operating recovery rate of 65.56% can be obtained. After mixed flotation, the grade of barite in the tailings is 10.94%, and the operating recovery rate of barite is 98.76%.
[0035] After the mixed concentrate has gone through the high-gradient strong magnetic separation process of one roughing and two sweeping, rare earth and fluorite can be effectively separated. The mineral processing technical indicators of fluorite concentrate are: operating yield is 92.58%, CaF2 grade is 95.42%, and CaF2 operating recovery rate is 96.82%; the mineral processing technical indicators of rare earth concentrate are: operating yield is 7.42%, TREO grade is 56.40%, and TREO operating recovery rate is 69.55%.
[0036] After the mixed flotation tailings undergo a shaking table gravity separation process of one coarse, two fine and one sweep, a qualified barite concentrate product with an operating yield of 8.40%, a BaSO4 grade of 96.01% and a BaSO4 operating recovery rate of 73.73% can be obtained. The barite content in the tailings meets the sulfur trioxide requirements of ordinary Portland cement raw materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The figure is a schematic diagram of the fineness test process of the rare earth and fluorite mixed flotation grinding of the present invention.
[0038] Figure 2 The present invention is a schematic diagram of the test flow of the dosage of sodium carbonate for the roughing of rare earth and fluorite mixed flotation.
[0039] Figure 3 The present invention is a schematic diagram of the test flow of the amount of water glass used in the roughing of rare earth and fluorite mixed flotation.
[0040] Figure 4 The figure is a schematic diagram of the test flow of the dosage of barite inhibitor in the roughing of rare earth and fluorite mixed flotation of the present invention.
[0041] Figure 5 The figure is a schematic diagram of the test flow of the dosage of the collector for the roughing of rare earth and fluorite mixed flotation of the present invention.
[0042] Figure 6 The figure is a schematic diagram of the open circuit test flow of the rare earth and fluorite mixed flotation of the present invention.
[0043] Figure 7 The figure is a schematic diagram of the closed-circuit test process of rare earth and fluorite mixed flotation of the present invention.
[0044] Figure 8 The figure is a schematic diagram of the quality flow of the closed-circuit test of mixed flotation of rare earth and fluorite of the present invention.
[0045] Fig. 9 The present invention is a schematic diagram of the process flow of the flotation concentrate rare earth and fluorite strong magnetic separation test.
[0046] Fig.10 The present invention is a schematic diagram of the test flow of the shaking table gravity separation of rare earth and fluorite mixed flotation tailings.
[0047] Fig.11 The present invention is a process flow chart of a mineral processing method for recovering rare earth, fluorite and barite from rare earth tailings.
[0048] Explanation of the attached table
[0049] Table 1 is the results of multiple chemical analyses of rare earth tailings of the present invention.
[0050] Table 2 shows the test results of the rare earth and fluorite mixed flotation grinding fineness of the present invention.
[0051] Table 3 shows the test results of the dosage of sodium carbonate in the roughing of rare earth and fluorite mixed flotation of the present invention.
[0052] Table 4 is the test results of the dosage of water glass in the roughing of rare earth and fluorite mixed flotation of the present invention.
[0053] Table 5 shows the test results of the dosage of barite inhibitor in the roughing of rare earth and fluorite mixed flotation of the present invention.
[0054] Table 6 is the test results of the dosage of collector for the roughing of rare earth and fluorite mixed flotation of the present invention.
[0055] Table 7 shows the open circuit test results of the rare earth and fluorite mixed flotation of the present invention.
[0056] Table 8 shows the closed-circuit test results of rare earth and fluorite mixed flotation in the present invention.
[0057] Table 9 shows the test results of strong magnetic separation of rare earth and fluorite in flotation concentrate of the present invention.
[0058] Table 10 shows the real-time indicators of the non-magnetic mineral products of the present invention.
[0059] Table 11 shows the technical indicators of the magnetic mineral products of the present invention.
[0060] Table 12 shows the test results of the shaker table gravity separation of rare earth and fluorite mixed flotation tailings of the present invention.
[0061] Table 13 shows the technical indicators of the barite concentrate product of the present invention. DETAILED DESCRIPTION
[0062] The present invention is now further described with reference to the accompanying drawings and attached tables.
[0063] See also Figure 1-10 , Appendix 1-13, the present invention provides a beneficiation process for recovering rare earth, fluorite and barite from rare earth tailings, comprising the following steps:
[0064] As shown in Table 1, chemical multi-line analysis was performed on the rare earth tailings.
[0065] Table 1 Results of multiple chemical analyses of rare earth tailings
[0066] project <![CDATA[Al2O3]]> <![CDATA[BaSO4]]> <![CDATA[CaCO3]]> <![CDATA[CaF2]]> CaO <![CDATA[K2O]]> MgO Mo content(%) 9.3 1.44 4 7.95 6.11 1.78 0.85 0.0212 project <![CDATA[Na2O]]> <![CDATA[P2O5]]> Pb <![CDATA[SiO2]]> <![CDATA[SrSO4]]> <![CDATA[TFe2O3]]> <![CDATA[TiO2]]> TREO content(%) 1.83 0.054 0.0645 64.54 0.045 1.08 0.26 0.57
[0067] like Figure 1 As shown, S1, rare earth and fluorite mixed flotation grinding fineness test:
[0068] The grinding concentration is 62.5%. Sodium carbonate 2000g / t is stirred for 3min, water glass 2000g / t is stirred for 3min, inhibitor TJ-1 200g / t is stirred for 3min, collector LT-1 600g / t is stirred for 2min, and then rough selection is carried out for 5min to obtain concentrate and tailings. It is confirmed that when the grinding fineness is -200 mesh accounting for 80%, the concentrate product indicators obtained are better.
[0069] Table 2 Test results of rare earth and fluorite mixed flotation grinding fineness
[0070]
[0071] like Figure 2 As shown, S2, the dosage test of sodium carbonate for roughing of rare earth and fluorite mixed flotation:
[0072] The grinding concentration is 62.5%, the grinding fineness is -200 mesh accounting for 80%, and 2000g / t of water glass is used for stirring for 3 minutes, the inhibitor TJ-1 200g / t is used for stirring for 3 minutes, and the collector LT-1 600g / t is used for stirring for 2 minutes and then roughing for 5 minutes. It is determined that when the amount of sodium carbonate used in the roughing of rare earth and fluorite mixed flotation is 1500g / t, the concentrate product indicators obtained are better.
[0073] Table 3 Test results of sodium carbonate dosage for roughing of rare earth and fluorite mixed flotation
[0074]
[0075] like Figure 3 As shown in S3, the water glass dosage test for the roughing of rare earth and fluorite mixed flotation:
[0076] Using the S2 method, water glass was set as a variable, and sodium carbonate was set to 1500g / t. It was determined that when the dosage of water glass in the roughing of rare earth and fluorite mixed flotation was 2000g / t, the indicators of the obtained concentrate product were better.
[0077] Table 4 Test results of water glass dosage for roughing of rare earth and fluorite mixed flotation
[0078]
[0079]
[0080] like Figure 4 As shown in S4, the test of the dosage of barite inhibitor in the roughing of rare earth and fluorite mixed flotation:
[0081] Using the S3 method, the inhibitor TJ-1 was set as a variable, and the water glass was set to 2000g / t. It was determined that when the dosage of the roughing inhibitor TJ-1 in the rare earth and fluorite mixed flotation was 200g / t, the concentrate product indicators obtained were better.
[0082] Table 5 Test results of barite inhibitor dosage in roughing of rare earth and fluorite mixed flotation
[0083]
[0084]
[0085] like Figure 5 As shown, S5, the roughing collector dosage test of rare earth and fluorite mixed flotation:
[0086] Using the S4 method, the collector LT-1 was set as a variable, and the inhibitor TJ-1 was set to 200g / t. It was determined that when the dosage of the collector LT-1 in the roughing of rare earth and fluorite mixed flotation was 800g / t, the concentrate product indicators obtained were better.
[0087] Table 6 Test results of collector dosage for mixed flotation of rare earth and fluorite
[0088]
[0089] like Figure 6As shown, S6, open circuit test of rare earth and fluorite mixed flotation:
[0090] S6-1, grinding concentration is 62.5%, grinding fineness is -200 mesh accounting for 80%, sodium carbonate 1500g / t is used for stirring for 3min, water glass 2000g / t is used for stirring for 3min, inhibitor TJ-1 200g / t is used for stirring for 3min, collector LT-1800g / t is used for stirring for 2min and then roughing for 5min;
[0091] S6-2, after roughing S6-1, select the first concentrate, stir with 800g / t of water glass for 3 minutes to obtain the second concentrate and the fourth medium ore; stir the second concentrate with 400g / t of water glass for 3 minutes to obtain the third concentrate and the third medium ore; stir the third concentrate with 200g / t of water glass for 3 minutes to obtain the fourth concentrate and the second medium ore; select the fourth concentrate again to obtain the concentrate and the first medium ore;
[0092] S6-3, after roughing S6-1, stir with 800 sodium carbonate for 3 minutes, stir with 1000 water glass for 3 minutes, stir with inhibitor TJ-1100 for 3 minutes, stir with collector LT-1 400 for 2 minutes, and then scavenge for 4 minutes to obtain the medium ore Wuhe tailings;
[0093] According to the results of the open circuit test, after an open circuit test of one roughing, one scavenging and four finishing, a mixed concentrate with an operating yield of 3.45%, a TREO grade of 6.28%, a CaF2 grade of 92.32%, a TREO operating recovery rate of 38.03%, and a CaF2 operating recovery rate of 40.09% can be obtained. After scavenging, the TREO grade in the tailings is 0.15%, and the CaF2 grade is 1.21%.
[0094] Table 7 Open circuit test results of rare earth and fluorite mixed flotation
[0095]
[0096] like Figure 7 As shown, S7, rare earth and fluorite mixed flotation closed circuit test:
[0097] S7-1, grinding concentration is 62.5%, grinding fineness is -200 mesh content is 80%, sodium carbonate 1500 is used for stirring for 3 minutes, water glass 2000 is used for stirring for 3 minutes, inhibitor TJ-1 200 is used for stirring for 3 minutes, collector LT-1 600 is used for stirring for 2 minutes and then roughing for 5 minutes;
[0098] S7-2, after roughing S7-1, select the first concentrate, stir with water glass 800 for 3 minutes to obtain select the second concentrate and the middle ore five; stir the second concentrate with water glass 400 for 3 minutes to obtain the third concentrate and the middle ore four; stir the third concentrate with water glass 200 for 3 minutes to obtain the fourth concentrate and the middle ore three; stir the fourth concentrate with water glass 100 for 3 minutes to obtain the fifth concentrate and the middle ore two; select the fifth concentrate again to obtain the concentrate and the middle ore one;
[0099] S7-3, after roughing S7-1, stir with 800 sodium carbonate for 3 minutes, stir with 1000 water glass for 3 minutes, stir with inhibitor TJ-1100 for 3 minutes, stir with collector LT-1 300 for 2 minutes, and then scavenge for 4 minutes to obtain the medium ore Liuhe tailings;
[0100] S7-4, mixing the intermediate ore 5 and the intermediate ore 6 obtained in S7-2 and S7-3 and then entering the step S7-1 again;
[0101] S7-5, returning the medium ore No. 4 in S7-2 to the step of selecting No. 1 in S7-2;
[0102] S7-6, returning the medium ore 3 in S7-2 to the step of selecting the second in S7-2;
[0103] S7-7, returning the medium ore 2 in S7-2 to the step of fine selection 3 in S7-2;
[0104] S7-8, returning the medium ore 1 in S7-2 to the step of selecting 4 in S7-2;
[0105] According to the results of the closed-circuit test, after a closed-circuit test of one roughing, one sweeping and five refining, a mixed concentrate with an operating yield of 5.71%, a TREO grade of 5.92%, a CaF2 grade of 91.24%, a TREO operating recovery rate of 59.32%, and a CaF2 operating recovery rate of 65.56% can be obtained, and the TREO grade in the tailings is 0.25%, and the CaF2 grade is 2.90%.
[0106] Table 8 Closed-circuit test results of rare earth and fluorite mixed flotation
[0107]
[0108] like Fig. 9 As shown, S8, flotation concentrate rare earth, fluorite strong magnetic separation test:
[0109] The flotation concentrate is subjected to a strong magnetic roughing separation with a magnetic field strength of 1.3T to obtain magnetic materials, and then subjected to a strong magnetic sweeping separation with a magnetic field strength of 1.3T to obtain magnetic materials, and then subjected to a strong magnetic sweeping separation with a magnetic field strength of 1.3T to obtain magnetic materials and non-magnetic materials;
[0110] Table 9 Results of the strong magnetic separation test of rare earth and fluorite in flotation concentrate
[0111]
[0112] As shown in Table 10, the non-magnetic mineral products obtained by the strong magnetic separation of rare earth and fluorite flotation concentrates meet the quality requirements of the third grade of fluorite concentrate national standard (GB5690-1985).
[0113] Table 10 Technical indicators of non-magnetic mineral products
[0114]
[0115]
[0116] Table 11 Technical indicators of magnetic mineral products
[0117] project TREO F CaO <![CDATA[P2O5]]> TFe Moisture content(%) 56.40 7.52 1.32 0.38 1.35 0.17
[0118] like Fig.10 S9, a rare earth and fluorite mixed flotation tailings gravity separation test:
[0119] After the mixed flotation tailings are roughly separated by shaking table gravity separation, tailings are obtained by shaking table gravity separation concentration 1, and then concentrate and tailings are obtained by bed gravity separation concentration 2.
[0120] Table 12 Test results of shaking table gravity separation of rare earth and fluorite mixed flotation tailings
[0121] product Yield (%) <![CDATA[BaSO4 grade (%)]]> <![CDATA[Recovery rate of BaSO4 (%)]]> Concentrate 1.20 96.01 68.58 Tailings 98.80 0.53 31.42 Feeding 100.00 1.68 100.00
[0122] As shown in Table 13, the barite concentrate obtained by the shaking table gravity separation of the rare earth and fluorite mixed flotation tailings meets the quality requirements of the national standard for barite powder for drilling fluid (GB / 5005-2001).
[0123] Table 13 Technical indicators of barite concentrate products
[0124]
[0125] The above are only preferred embodiments of the present invention, which are only used to help understand the method and core idea of the present application. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the idea of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
[0126] The present invention solves the problem in the prior art that fluorite or barite is often treated as solid waste and its value of secondary development and recycling is ignored, resulting in waste of resources. The invention realizes efficient recovery of rare earth and fluorite through a closed circuit of one coarse, five fine and two sweeps, and separation of rare earth and fluorite is realized through high-gradient strong magnetic separation of one coarse and two sweeps. The tailings also realize efficient recovery of barite through the center of the shaking table, providing practical and effective help for maximizing resource utilization.
Claims
1. A beneficiation process for recovering rare earth, fluorite and barite from rare earth tailings, It is characterized in that The following steps are involved: S1, rare earth and fluorite mixed flotation grinding fineness test: The grinding concentration is 62.5%. Sodium carbonate 2000g / t is used for stirring for 3min, water glass 2000g / t is used for stirring for 3min, inhibitor TJ-1 200g / t is used for stirring for 3min, collector LT-1 600g / t is used for stirring for 2min, and then roughing for 5min is performed to obtain concentrate and tailings. It is confirmed that the best rare earth and fluorite mixed flotation grinding fineness is -200 mesh accounting for 80%; S2, Sodium carbonate dosage test for roughing of rare earth and fluorite mixed flotation: The grinding concentration is 62.5%, the grinding fineness is -200 mesh accounting for 80%, and 2000g / t of water glass is used for stirring for 3min, the inhibitor TJ-1 200g / t is used for stirring for 3min, and the collector LT-1 600g / t is used for stirring for 2min and roughing for 5min to obtain the concentrate and tailings, and it is confirmed that the optimal sodium carbonate dosage for the roughing of rare earth and fluorite mixed flotation is 1500g / t; S3, water glass dosage test for roughing of rare earth and fluorite mixed flotation: The S2 method was adopted, with water glass set as a variable and sodium carbonate set at 1500 g / t, to obtain concentrate and tailings, and it was confirmed that the optimal water glass dosage for the roughing of rare earth and fluorite mixed flotation was 2000 g / t; S4, test on the dosage of barite inhibitor in the roughing of rare earth and fluorite mixed flotation: The S3 method was adopted, the inhibitor TJ-1 was set as a variable, the water glass was set to 2000g / t, the concentrate and tailings were obtained, and the optimal dosage of the barite inhibitor TJ-1 for the roughing of rare earth and fluorite mixed flotation was confirmed to be 200g / t; S5, rare earth and fluorite mixed flotation roughing collector dosage test: The S4 method was used to set the collector LT-1 as a variable and the inhibitor TJ-1 as 200 g / t to obtain concentrate and tailings, and it was confirmed that the optimal dosage of the collector LT-1 for the roughing of rare earth and fluorite mixed flotation was 800 g / t. S6, open circuit test of rare earth and fluorite mixed flotation: S6-1, grinding concentration is 62.5%, grinding fineness is -200 mesh accounting for 80%, sodium carbonate 1500g / t is used for stirring for 3min, water glass 2000g / t is used for stirring for 3min, inhibitor TJ-1 200g / t is used for stirring for 3min, collector LT-1 800g / t is used for stirring for 2min, and then roughing for 5min to obtain mixed rough concentrate and roughing tailings; S6-2, the mixed coarse concentrate obtained in S6-1 is subjected to concentration one, and after stirring with 800 g / t of water glass for 3 minutes, a concentration two and a medium ore 4 are obtained; after stirring with 400 g / t of water glass for 3 minutes, a concentration three and a medium ore 3 are obtained; after stirring with 200 g / t of water glass for 3 minutes, a concentration four and a medium ore 2 are obtained; after concentrating the concentration four again, a concentrate and a medium ore 1 are obtained; S6-3, the rough tailings obtained in S6-1 were scavenged by stirring with 800 g / t of sodium carbonate for 3 min, 1000 g / t of water glass for 3 min, 100 g / t of inhibitor TJ-1 for 3 min, 400 g / t of collector LT-1 for 2 min, and then scavenged for 4 min to obtain the middling ore 5 and tailings; S7, Closed-circuit test of rare earth and fluorite mixed flotation: S7-1, grinding concentration is 62.5%, grinding fineness is -200 mesh accounting for 80%, sodium carbonate 1500g / t is used for stirring for 3min, water glass 2000g / t is used for stirring for 3min, inhibitor TJ-1 200g / t is used for stirring for 3min, collector LT-1 600g / t is used for stirring for 2min and then roughing for 5min; S7-2, after roughing S7-1, select the first concentrate, stir with 800g / t of water glass for 3min to obtain select the second concentrate and the middle ore five; stir with 400g / t of water glass for 3min to obtain select the third concentrate and the middle ore four; stir with 200g / t of water glass for 3min to obtain select the fourth concentrate and the middle ore three; stir with 100g / t of water glass for 3min to obtain select the fifth concentrate and the middle ore two; select the fifth concentrate again to obtain the concentrate and the middle ore one; S7-3, after roughing S7-1, stir with 800g / t of sodium carbonate for 3min, stir with 1000g / t of water glass for 3min, stir with 100g / t of inhibitor TJ-1 for 3min, stir with 300g / t of collector LT-1 for 2min, and then scavenge for 4min to obtain the medium ore Liuhe tailings; S7-4, mixing the intermediate ore 5 and the intermediate ore 6 obtained in S7-2 and S7-3 and then entering the step S7-1 again; S7-5, returning the medium ore No. 4 in S7-2 to the step of selecting No. 1 in S7-2; S7-6, returning the medium ore 3 in S7-2 to the step of selecting the second in S7-2; S7-7, returning the medium ore 2 in S7-2 to the step of fine selection 3 in S7-2; S7-8, returning the medium ore 1 in S7-2 to the step of selecting 4 in S7-2; S8, Mixed flotation concentrate rare earth, fluorite strong magnetic separation test: The mixed flotation concentrate is subjected to a strong magnetic roughing separation with a magnetic field strength of 1.3T to obtain magnetic and non-magnetic materials, the non-magnetic materials are subjected to a strong magnetic sweeping separation with a magnetic field strength of 1.3T to obtain strong magnetic sweeping separation first intermediate ore and strong magnetic sweeping separation first tailings, and the strong magnetic sweeping separation tailings are subjected to a strong magnetic sweeping separation second with a magnetic field strength of 1.3T to obtain strong magnetic sweeping separation second intermediate ore and strong magnetic sweeping separation second tailings; S9, rare earth and fluorite mixed flotation tailings gravity separation test: After the mixed flotation tailings are roughly separated by shaking table gravity separation, tailings are obtained by shaking table gravity separation concentration 1, and then concentrate and tailings are obtained by bed gravity separation concentration 2.