Preparation method of hydroxyapatite powder with high purity and different strengths

By processing calcium oxide and phosphoric acid through steps such as stirring and high-speed shearing emulsification under alkaline conditions, combined with segmented calcination, the problems of low purity and complex process of hydroxyapatite powder in the existing technology are solved, and high purity and hardness are achieved. The preparation of controllable hydroxyapatite powder is suitable for industrial production.

CN118851114AActive Publication Date: 2024-10-29SICHUAN MIANYANG XINGHEYI NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202410617569.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-17
Publication Date
2024-10-29
Estimated Expiration
2044-05-17

AI Technical Summary

Technical Problem

The existing synthesis method of hydroxyapatite powder results in low product purity, affects biocompatibility and strength, and the process is complex, consuming water and energy, making it difficult to meet the needs of industrial production.

Method used

Calcium oxide and phosphoric acid are stirred under alkaline conditions, high-speed shearing emulsification, aging, filter press, drying and segmented calcination are used to control process parameters, avoid the generation of by-products, and form high-purity products of different shapes and hardnesses. Hydroxyapatite.

Benefits of technology

It achieves the preparation of hydroxyapatite powder with high purity and controllable hardness, simplifies the process, saves water, reduces production costs, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851114A_ABST
    Figure CN118851114A_ABST
Patent Text Reader

Abstract

The invention relates to the field of novel materials, in particular to a preparation method of hydroxyapatite powder with high purity and controllable hardness, which comprises the following steps: adding water into calcium oxide to prepare a calcium hydroxide suspension, and heating the calcium hydroxide suspension; heating, concentrating and dehydrating phosphoric acid; stirring the heated calcium hydroxide suspension and the phosphoric acid with improved polymerization degree under an alkaline condition, and fully and uniformly mixing; carrying out high-speed shearing emulsification on the mixture after the reaction is finished; aging the mixture subjected to shearing emulsification; carrying out filter pressing on the aged mixture, and drying a filter cake; and carrying out segmented calcination on the dried solid to obtain hydroxyapatite with different shapes. The process is simple and easy to operate, the raw materials are low in price and easy to obtain, the cost is low, the cost performance is high, and the method is very suitable for large-scale process production and is improvement of hydroxyapatite prepared by a chemical precipitation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of new materials (ceramics), and in particular to a method for preparing high-purity hydroxyapatite powders of different strengths. Background Art

[0002] Hydroxyapatite is currently recognized as a new type of ceramic material with good biocompatibility and osteoconductivity, that is, biosoluble. It is the main component of human and animal bones, teeth, and tusks. With the advancement of science and technology and the continuous improvement of people's understanding, many research results show that hydroxyapatite is a non-toxic, non-carcinogenic, non-side effect, and biocompatible bioactive material. People have also found that hydroxyapatite has solid alkaline properties and strong polymer exchange capacity. Therefore, it is widely used in catalytic carriers and polymer fields (industrial water and domestic water defluorination. At the same time, it can also have ion and temperature sensitivity, humidity sensitivity effects, and passivate heavy metal cadmium ions in soil improvement. Therefore, it is also a green, environmentally friendly, degradable material and intelligent material. It has better lipophilicity, hydrophilicity, and protein adsorbent. It is also used in different polymer plastic composites to resist high temperature, shear, and increase mechanical strength. With the expansion of application fields, the requirements for its performance and product purity are getting higher and higher.

[0003] Hydroxyapatite is not a natural mineral, but mainly relies on artificial synthesis. At present, the synthesis methods of hydroxyapatite powder are generally divided into two types: wet method and dry method. In addition, it can be obtained from animal bones. The hydroxyapatite obtained by these methods has low product purity, which in turn affects the biocompatibility and product strength of hydroxyapatite. The performance cannot meet the needs of the application market. In the process field, hydroxyapatite is prepared to better exert product performance, which cannot provide guarantees for product upgrades. In order to obtain purer products, these production methods save a lot of water washing, acid washing, alcohol washing and other processes in the process. This will lead to a large amount of wastewater and waste residue that deviates from the current national environmental requirements. Either the production conditions are harsh, the process needs to meet high temperature and high pressure conditions, and the risk factor increases. These conditions increase production costs, and the process equipment is complex, difficult to control, and industrialized production. Summary of the invention

[0004] The present application provides a method for preparing high-purity hydroxyapatite powders of different strengths to solve the technical problems in the prior art.

[0005] In a first aspect, the present application provides a method for preparing high-purity hydroxyapatite powder with controllable hardness, comprising the following steps:

[0006] S1, adding water to calcium oxide to prepare a calcium hydroxide suspension, and heating the calcium hydroxide suspension; heating, concentrating and dehydrating phosphoric acid;

[0007] S2, stirring the heated calcium hydroxide suspension and the phosphoric acid with increased polymerization degree under alkaline conditions to fully mix them;

[0008] S3, subjecting the mixture after the reaction to high-speed shear emulsification;

[0009] S4, aging the mixture after shear emulsification for 4 to 8 hours;

[0010] S5, filtering the mixture after aging, and drying the filter cake;

[0011] S6. The dried solid is calcined in stages to obtain hydroxyapatite of different shapes.

[0012] Optionally, the concentration of the calcium hydroxide suspension is 8% to 12% and is heated to 60 to 70°C.

[0013] Optionally, the concentration of the phosphoric acid is 85%, and the degree of polymerization is increased to 8-10 after treatment.

[0014] Optionally, the mass ratio of the phosphoric acid to the calcium hydroxide suspension is 1:3.

[0015] Optionally, a phosphorus-containing pH alkaline stabilizer is added to the reaction system after the reaction is completed.

[0016] Optionally, the drying temperature is 100° C. and the drying time is 0.5 to 1 hour.

[0017] Optionally, the staged calcination comprises the following steps:

[0018] The temperature range is controlled at 100-200°C and calcined for 2 hours to obtain amorphous needle-shaped hydroxyapatite;

[0019] The temperature range is controlled at 200-600°C and calcined for 4 hours to obtain cylindrical hydroxyapatite;

[0020] The temperature range is controlled at 600-1250°C and calcined for 6 hours to obtain spherical hydroxyapatite.

[0021] Optionally, the Mohs hardness of the calcined hydroxyapatite is 5.8 to 6.8.

[0022] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0023] 1. The raw materials used in the present invention are cheap and easy to obtain, the preparation process is simple, the process parameters are simple and easy to control, and there is no need to add too much auxiliary agent and a large amount of water washing, acid washing, and alcohol washing process. It is environmentally friendly and saves water, achieving water recycling, which is both economical and environmentally friendly.

[0024] 2. The present invention adjusts the ratio of raw materials and strictly controls the parameters of each process flow, thereby avoiding incomplete reaction and the generation of other calcium phosphates, thereby ensuring the high purity of hydroxyapatite.

[0025] 3. The present invention forms different crystal forms of hydroxyapatite at different temperatures by calcining at different temperatures, thereby changing the mechanical properties of hydroxyapatite, different hardness and crystal shape, and also increasing the hardness of the product to 5.8-6.8 (Mohs hardness).

[0026] 4. The technical solution of the present invention can produce 10,000 tons of hydroxyapatite annually, which has good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0029] Figure 1 is a process flow chart of the present invention;

[0030] Figure 2 is the X-ray diffraction pattern of hydroxyapatite;

[0031] Figure 3 This is an electron microscope image of spherical hydroxyapatite;

[0032] Figure 4 This is an electron microscope image of needle-shaped hydroxyapatite;

[0033] Figure 5 This is an electron microscope image of rod-shaped hydroxyapatite;

[0034] Figure 6 This is the SEM photo of the microscopic morphology of hydroxyapatite powder;

[0035] Figure 7 This is an EDS composition scanning photo of the surface of hydroxyapatite powder;

[0036] Figure 8 is the EDS element percentage curve of hydroxyapatite powder surface;

[0037] Fig. 9 Selected diagram of chemical elements for hydroxyapatite powder;

[0038] Fig.10 The XRD diffraction pattern of hydroxyapatite powder is compared with the theoretical PDF card;

[0039] Fig.11 This is the XRD phase structure analysis diagram of hydroxyapatite powder;

[0040] Fig.12 This is a comparison chart of wear resistance test. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0042] In one embodiment of the present application, a method for preparing high-purity hydroxyapatite powder with controllable hardness comprises the following steps:

[0043] S1, adding water to calcium oxide to prepare a calcium hydroxide suspension, and heating the calcium hydroxide suspension; heating, concentrating and dehydrating phosphoric acid in a heating dehydration tank;

[0044] S2. In a heat-insulating reactor, the heated calcium hydroxide suspension and the phosphoric acid with an increased degree of polymerization are stirred under alkaline conditions to be fully mixed;

[0045] S3, subjecting the mixture after the reaction to high-speed shear emulsification in a high-speed shear emulsification device;

[0046] S4, aging the mixture after shear emulsification in an aging tank for 4 to 8 hours;

[0047] S5, filtering the mixture after aging through a fully automatic liquid press to achieve solid-liquid separation, drying the filter cake, and the mother liquor enters the circulating water use system for calcium oxide treatment;

[0048] S6. The dried solid is calcined in stages to obtain hydroxyapatite of different shapes and hardnesses.

[0049] In the present application, lime / calcium oxide and phosphoric acid are used as raw materials, and there is no need to adjust the pH value and the related aging time, and no need for ion water washing, acid washing, and alcohol washing. After calcium hydroxide slurry is made by calcium oxide / limestone, it is titrated and neutralized with a certain concentrated phosphoric acid, and then dehydrated, dried, and calcined to obtain micron-sized hydroxyapatite powder. The whole process is simple and easy to control, will not cause pollution to the environment, is economical and environmentally friendly, and is suitable for large-scale process production. It is an improvement and improvement of the chemical precipitation method for producing hydroxyapatite.

[0050] As an optional embodiment, the concentration of the calcium hydroxide suspension is 8% to 12% and is heated to 60 to 70°C.

[0051] In the present application, the concentration of the calcium hydroxide suspension is regulated and heated to prevent the formation of other by-products such as calcium phosphates.

[0052] As an optional embodiment, the concentration of phosphoric acid is 85%, and the degree of polymerization is increased to 8-10 after treatment.

[0053] In the present application, 85% of phosphoric acid is dehydrated to make its polymerization degree reach 8-10, thereby reducing the hydrolysis reaction rate and further avoiding the generation of by-products such as dicalcium hydrogen phosphate and monocalcium phosphate.

[0054] As an optional embodiment, the mass ratio of the phosphoric acid to the calcium hydroxide suspension is 1:3.

[0055] In the present application, the mass ratio of phosphoric acid and calcium hydroxide suspension is limited, and the two react according to the following reaction equation: 10Ca 2+ +6PO4 3- +2OH - →Ca 10 (Po4)5(OH)2, reducing the formation of by-products.

[0056] As an optional embodiment, a phosphorus-containing pH alkaline stabilizer is added to the reaction system after the reaction is completed.

[0057] In the present application, the pH of the reaction system is stabilized within a certain range to avoid the generation of other dicalcium hydrogen phosphate and monocalcium phosphate.

[0058] As an optional embodiment, the staged calcination comprises the following steps:

[0059] The temperature range is controlled at 100-200°C and calcined for 2 hours to obtain amorphous needle-shaped hydroxyapatite;

[0060] The temperature range is controlled at 200-600°C and calcined for 4 hours to obtain cylindrical hydroxyapatite;

[0061] The temperature range is controlled at 600-1250°C and calcined for 6 hours to obtain spherical hydroxyapatite.

[0062] In the present application, according to the different uses of hydroxyapatite, the calcination temperature and calcination time are controlled so that the shapes of the product particles are three different shapes of products: amorphous needle-shaped, cylindrical, and spherical. Products of different shapes have application performances of different strengths and are used in different industrial fields.

[0063] As an optional embodiment, the Mohs hardness of the calcined hydroxyapatite is 5.8-6.8.

[0064] In the present application, the Mohs hardness of the hydroxyapatite prepared in the present application is 5.8 to 6.8, and it has a wide range of application performance. Applying it to the coating can greatly improve the wear resistance of the coating.

[0065] Example 1

[0066] A method for preparing high-purity hydroxyapatite powder with controllable hardness comprises the following steps:

[0067] S1. Add water to calcium oxide to prepare a calcium hydroxide suspension with a concentration of 8% to 12%, and heat the calcium hydroxide suspension to 60 to 70° C.; heat, concentrate, and dehydrate 85% phosphoric acid to increase its polymerization degree to 8 to 10;

[0068] S2, adding the heated calcium hydroxide suspension and the phosphoric acid with an increased degree of polymerization into a heat-insulating reactor in a mass ratio of 3:1, stirring under alkaline conditions, mixing thoroughly, and adding a phosphorus-containing pH alkaline stabilizer after obtaining the desired pH value;

[0069] S3, subjecting the mixture after the reaction to high-speed shear emulsification;

[0070] S4, aging the mixture after shear emulsification for 4 to 8 hours;

[0071] S5, filtering the mixture after aging, and drying the filter cake at 100° C. for 0.5 to 1 h;

[0072] S6, calcining the dried solid in stages;

[0073] The temperature range is controlled at 100-200°C and calcined for 2 hours to obtain amorphous needle-shaped hydroxyapatite;

[0074] The temperature range is controlled at 200-600°C and calcined for 4 hours to obtain cylindrical hydroxyapatite;

[0075] The temperature range is controlled to be 600-1250°C and calcined for 6 hours to obtain spherical hydroxyapatite;

[0076] The Mohs hardness of the calcined hydroxyapatite is 5.8-6.8.

[0077] The hydroxyapatite prepared by the present invention was tested by a D / Max-2550pc multi-product X-ray diffractometer according to JY / T009-1996 General Rules for Rotating Target Polycrystalline X-ray Diffraction Method. The test results are as follows: Figure 1 .Depend on Figure 1 It can be seen that the composition of the hydroxyapatite prepared by the present invention is Ca5(PO4)3(OH), the structure is hexagonal crystal, and the space group is P63 / m(176 # )

[0078] Depend on Figure 6 It can be seen that the hydroxyapatite produced by the present invention is in the form of particle clusters (ab) or amorphous structure (see Figure cf), wherein the diameter of a single cluster is about 5 to 8 μm.

[0079] Depend on Figure 7-Figure 8 It can be seen that the hydroxyapatite produced by the present invention is mainly composed of C, O, P, Ca, Na, and Si elements, of which Ca content accounts for 39.95wt.%, P content accounts for 17.25wt.%, and O content accounts for 42.23wt.%; trace Na and Si elements account for 0.17wt.% and 0.32wt.%, respectively. Chemical elements are selected based on the elemental composition of the above energy spectrum and the basic elements that may be involved in the sample. H, C, N, O, Na, Si, P, and Ca elements are selected for this sample. Secondly, the PDF card library is selected. When "Minerals" is selected, it can be seen from the automatic analysis of S / M matching that in principle, the best option is preliminarily determined based on the smaller FOM value and the one-to-one correspondence of the three strongest peaks; but by comparing Fig.10 From the four theoretical PDF cards in the paper, we can see that the theoretical card Ca5(PO 4)3 In the diffraction angle range of 10°~90°, the three strongest peaks of F and theoretical cards Ca5(PO4)3OH and Ca5(PO4)3OH basically correspond to the diffraction peaks of the test sample. However, careful comparison and observation show that the diffraction peaks of the theoretical card Ca3(PO4)3OH and the test sample have the highest consistency. Combined with the component analysis of energy spectrum EDS, it was found that no F element was detected. Therefore, comprehensive analysis can determine that the test sample is Ca5(PO4)3OH in terms of phase structure.

[0080] Quartz sand and the hydroxyapatite prepared in this application were used to prepare samples for comparison and testing of the wear resistance of the paint film. The designed formula is shown in Table 1.

[0081] Resin 50 Additives 2 Solvents 30 Quartz sand / Hydroxyapatite 18 total 100

[0082] According to GB / T1768, the test was carried out using a TABER abrasion tester, a rubber grinding wheel CS-17, a paint film thickness of 40 microns, and 750g / 500r. The test results are shown in Fig.12 , indicating that hydroxyapatite has a relatively high Mohs hardness and adding it to the coating can significantly improve the wear resistance of the coating, and can be used as a wear-resistant functional filler.

[0083] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0084] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A method for preparing high-purity hydroxyapatite powder with controllable hardness, characterized in that: The following steps are involved: S1, adding water to calcium oxide to prepare a calcium hydroxide suspension, and heating the calcium hydroxide suspension; heating, concentrating and dehydrating phosphoric acid; S2, stirring the heated calcium hydroxide suspension and the phosphoric acid with increased polymerization degree under alkaline conditions to fully mix them; S3, subjecting the mixture after the reaction to high-speed shear emulsification; S4, aging the mixture after shear emulsification for 4 to 8 hours; S5, filtering the mixture after aging, and drying the filter cake; S6. The dried solid is calcined in stages to obtain hydroxyapatite of different shapes.

2. The method for preparing a high-purity hydroxyapatite powder with controllable hardness according to claim 1, characterized in that: The concentration of the calcium hydroxide suspension is 8% to 12%, and the suspension is heated to 60 to 70°C.

3. The method for preparing a high-purity hydroxyapatite powder with controllable hardness according to claim 1, characterized in that: The concentration of the phosphoric acid is 85%, and the degree of polymerization is increased to 8-10 after the treatment.

4. The method for preparing a high-purity hydroxyapatite powder with controllable hardness according to claim 1, characterized in that: The mass ratio of the phosphoric acid to the calcium hydroxide suspension is 1:

3.

5. The method for preparing a high-purity hydroxyapatite powder with controllable hardness according to claim 1, characterized in that: After the reaction is completed, a phosphorus-containing pH alkaline stabilizer is added to the reaction system.

6. The method for preparing a high-purity hydroxyapatite powder with controllable hardness according to claim 1, characterized in that: The drying temperature is 100°C and the drying time is 0.5 to 1 hour.

7. The method for preparing a high-purity hydroxyapatite powder with controllable hardness according to claim 1, characterized in that: The staged calcination includes the following steps: The temperature range is controlled at 100-200°C and calcined for 2 hours to obtain amorphous needle-shaped hydroxyapatite; The temperature range is controlled at 200-600°C and calcined for 4 hours to obtain cylindrical hydroxyapatite; The temperature range is controlled at 600-1250°C and calcined for 6 hours to obtain spherical hydroxyapatite.

8. The method for preparing a high-purity hydroxyapatite powder with controllable hardness according to claim 7, characterized in that: The Mohs hardness of the calcined hydroxyapatite is 5.8-6.8.

Citation Information

Patent Citations

  • Method for producing hydroxyapatite through waste phosphoric acid

    CN104528678A

  • Process for preparing modified hydroxy apatite powder

    CN1899957A

  • Process for preparing an aqueous suspension of hydroxyapatite

    DE4037103C1

  • Production of spherical hydroxyapatite

    JP1991083805A

  • Production method of hydroxyapatite crystal

    JP2015168605A

Cited By

  • Preparation method of hydroxyapatite

    CN120573661A