Na-site doped carbon-coated ferric sodium pyrophosphate as well as preparation method and application of Na-site doped carbon-coated ferric sodium pyrophosphate

By using Na-doped carbon to coat sodium ferric pyrophosphate in sodium-ion batteries, the diffusion channel of Na+ is expanded and the crystal structure is stabilized, thereby solving the problem of low rate performance of sodium-ion batteries and achieving high rate performance of the material. Improved cycle stability.

CN118851132APending Publication Date: 2024-10-29XIAN UNIV OF TECH +1

Patent Information

Application Number
CN202411035551.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The rate performance of sodium-ion batteries is low, which limits the further development of sodium-ion batteries.

Method used

Sodium ferric pyrophosphate is coated with Na-site doped carbon, whose chemical formula is AxByNa4-x-2yFe3(PO4)2P2O7/C. The diffusion channel of Na+ is expanded by introducing pillar ions at the Na site, and the crystal is stabilized through three-step heat treatment. structure, introducing carbon source to exert chelation effect and improve the electronic conductivity of the material.

Benefits of technology

The rate performance and cycle stability of the material are significantly improved, making it an excellent cathode material for sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851132A_ABST
    Figure CN118851132A_ABST
Patent Text Reader

Abstract

The invention discloses Na-site doped carbon-coated ferric sodium pyrophosphate as well as a preparation method and application thereof, belongs to the technical field of battery materials, and solves the problem of relatively low rate capability of a sodium ion battery in the prior art. The chemical formula of the Na-site doped carbon-coated pyrophosphate ferric sodium phosphate provided by the invention is A < x > B < y > Na < 4-x-2y > Fe < 3 > (PO4) < 2 > P < 2 > O < 7 > / C, wherein x is more than or equal to 0 and less than or equal to 0.2, y is more than or equal to 0 and less than or equal to 0.2, x + 2y is more than 0, A is one or a combination of more of Li, K, Rb and Cs, and B is Ca. According to the Na-site doped carbon-coated ferric sodium pyrophosphate provided by the invention, in-situ doping is carried out at the Na site to introduce pillar ions, expand a diffusion channel of Na < + > and improve the cycling stability, so that positive influence is generated on the electrochemical performance of the material, the material has excellent electrochemical performance, and the rate capability and the cycling stability of the material are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and more specifically to a Na-doped carbon-coated sodium iron pyrophosphate and a preparation method and application thereof. Background Art

[0002] Sodium iron pyrophosphate (Na4Fe3(PO4)2P2O7, denoted as NFPP), a cathode material for sodium ion batteries, has a high theoretical capacity (~129 mAh / g) and a high operating voltage (~3.1 V, Na + / Na) and low volume expansion (~4%), and is considered to be a very promising cathode material for sodium-ion batteries.

[0003] However, common NFPP generally has the problem of slow kinetic rate due to the large ionic radius of sodium ions, resulting in low rate performance, which restricts the further development of sodium-ion batteries. Summary of the invention

[0004] The present invention provides a Na-doped carbon-coated sodium iron pyrophosphate and a preparation method and application thereof, which are used to solve the problem of low rate performance of sodium ion batteries in the prior art.

[0005] In the first aspect, the present invention provides a Na-doped carbon-coated sodium iron pyrophosphate, whose chemical formula is A x B y Na 4-x-2y Fe3(PO4)2P2O7 / C; wherein 0≤x≤0.2, 0≤y≤0.2, and x+2y>0, A is one or a combination of Li, K, Rb, Cs, and B is Ca.

[0006] As a possible implementation, the particle size of the Na-doped carbon-coated sodium iron pyrophosphate provided by the present invention is 20 nm to 10 μm. Exemplarily, the particle size of the Na-doped carbon-coated sodium iron pyrophosphate provided by the present invention is 3 μm to 5 μm.

[0007] In a second aspect, the present invention provides a method for preparing Na-doped carbon-coated sodium iron pyrophosphate as described in any possible implementation of the first aspect, comprising the following steps: mixing and dissolving source A / source B, a sodium source, an iron source, a phosphorus source and a carbon source in water, and drying and grinding the resulting mixed solution in sequence to obtain a precursor; pre-calcining the precursor in an inert atmosphere at 200 to 400° C., grinding it twice and sintering it in two stages in an inert atmosphere in sequence to obtain the Na-doped carbon-coated sodium iron pyrophosphate; wherein, in the two stages, the temperature condition of the first stage is 200 to 400° C., and the temperature condition of the second stage is 500 to 700° C.

[0008] As a possible implementation, the A source / B source, the sodium source, the iron source, the phosphorus source and the carbon source described in the present invention refer to soluble salts; specifically, the A source is one or a combination of dihydrogen phosphate A, bicarbonate A, sulfuric acid A, chloric acid A, carbonate A, acetic acid A, and fluoride A, and the B source is one or a combination of dihydrogen phosphate B, bicarbonate B, sulfuric acid B, chloric acid B, carbonate B, acetic acid B, and fluoride B; and / or, the sodium source is one or a combination of sodium dihydrogen phosphate and disodium hydrogen phosphate; and / or, the iron source is one or a combination of ferric nitrate, ferrous acetate, ferrous oxalate and ferrous sulfate; and / or, the carbon source is one or a combination of citric acid, vitamin C, glucose and oxalic acid.

[0009] Exemplarily, the A source is dihydrogen phosphate A, the B source is dihydrogen phosphate B; and / or the sodium source is sodium dihydrogen phosphate; and / or the iron source is ferric nitrate; and / or the carbon source is citric acid.

[0010] As a possible implementation method, the ratio of the amount of substance of the A source / B source, the sodium source and the iron source is the ratio of the amount of substance of each element in the chemical formula; and / or, the ratio of the mass of the carbon source to the sum of the mass of the A source / B source, the sodium source, the iron source and the phosphorus source is 1:2 to 4.

[0011] Exemplarily, the ratio of the mass of the carbon source to the sum of the masses of the A source / B source, the sodium source, the iron source and the phosphorus source is 1:3.

[0012] As a possible implementation method, the mixed dissolution in water is stirred for 1 to 4 hours; and / or the drying method is spray drying or freeze drying, and the drying conditions are: inlet temperature 200 to 300°C, feed rate 500 to 1000 mL / h; and / or the inert atmosphere is one or a combination of nitrogen, argon and hydrogen; and / or the pre-calcination heating rate is 1 to 10°C / min, and the insulation time is 0.5 to 6 hours; and / or the heating rate of the first stage is 0.5 to 10°C / min, and the insulation time is 2 to 5 hours, and the heating rate of the second stage is 0.5 to 10°C / min, and the insulation time is 4 to 10 hours.

[0013] Exemplarily, the mixed dissolution in water is stirred for 2 hours; and / or the drying method is spray drying, and the drying conditions are: inlet temperature 260°C, feed rate 800mL / h; and / or the inert atmosphere is argon; and / or the sintering includes the following steps: first stage: heating to 300°C at a heating rate of 5°C / min, and keeping warm for 3 hours; second stage: heating to 550°C at a heating rate of 2°C / min, and keeping warm for 8 hours.

[0014] In the third aspect, the present invention provides the use of Na-doped carbon-coated sodium iron pyrophosphate described in any possible implementation of the first aspect or the Na-doped carbon-coated sodium iron pyrophosphate prepared by the preparation method described in any possible implementation of the second aspect in the preparation of positive electrode materials for sodium ion batteries.

[0015] In a fourth aspect, the present invention provides a sodium ion battery positive electrode material, comprising a conductive agent, a binder and an active substance, wherein the active substance comprises the Na-doped carbon-coated sodium iron pyrophosphate described in any possible implementation of the first aspect or the Na-doped carbon-coated sodium iron pyrophosphate prepared by the preparation method described in any possible implementation of the second aspect.

[0016] In a fifth aspect, the present invention provides a method for preparing the sodium ion battery positive electrode material described in the fourth aspect, comprising the following steps: dissolving the Na-doped carbon-coated sodium iron pyrophosphate, a conductive agent and a binder in a polar solvent at a mass ratio of 7 to 8:1 to 2:1; applying it on the battery positive electrode collector, and drying to obtain the Na ion battery positive electrode material.

[0017] As a possible implementation, the conductive agent is acetylene black; and / or the binder is polyvinylidene fluoride; and / or the polar solvent is N-methylpyrrolidone; and / or the mass ratio of the Na-doped carbon-coated sodium ferric pyrophosphate, the conductive agent and the binder is 7:2:1; and / or the battery positive electrode collector is aluminum foil; and / or the drying conditions are 90°C and 10 hours.

[0018] The Na-doped carbon-coated sodium iron pyrophosphate provided by the present invention is in-situ doped at the Na position to introduce pillar ions, thereby expanding the Na + The diffusion channel is opened, and the cycle stability is improved, which has a positive impact on the electrochemical properties of the material, making it have excellent electrochemical properties, effectively improving the rate performance and cycle stability of the material, and becoming a potential positive electrode material for sodium ion batteries.

[0019] The preparation method of Na-doped carbon-coated sodium ferric pyrophosphate provided by the present invention introduces pillar ions at the Na position, introduces a carbon source, and obtains the final desired Na-doped carbon-coated sodium ferric pyrophosphate through three-step heat treatment. In which, the introduction of pillar ions at the Na position can expand the Na +The diffusion channel is opened, and the cycle stability is improved, which has a positive impact on the electrochemical properties of the material, making it have excellent electrochemical properties; the introduction of carbon source can play a chelating role, fully coordinate the complex metal ions, make the material particle size more uniform, and has the effect of reducing trivalent iron and enhancing the electronic conductivity of the material, thereby improving the electronic conductivity of the material; the three-step heat treatment can stabilize the crystal structure, reduce structural stress, and enhance structural reversibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 XRD diagram of the Na-doped carbon-coated sodium iron pyrophosphate used as a positive electrode material for a battery provided in an embodiment of the present invention.

[0022] Figure 2 This is a SEM microscopic morphology of the Na-doped carbon-coated sodium iron pyrophosphate provided in an embodiment of the present invention as a battery positive electrode material.

[0023] Figure 3 The discharge specific capacity results of button cell I, button cell XII and button cell XIII provided in the embodiments of the present invention are shown.

[0024] Figure 4 The charge and discharge curves of button battery I, button battery XII and button battery XIII provided in the embodiments of the present invention.

[0025] Figure 5 The discharge specific capacity results of button cell I, button cell XII and button cell XIII provided in the embodiments of the present invention are shown. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In order to solve the problem of low rate performance of sodium ion batteries in the prior art, the present invention provides a Na-doped carbon-coated sodium iron pyrophosphate and a preparation method and application thereof. The chemical formula of the Na-doped carbon-coated sodium iron pyrophosphate is A x By Na 4-x-2y Fe3(PO4)2P2O7 / C; wherein 0≤x≤0.2, 0≤y≤0.2, and x+2y>0, A is one or a combination of Li, K, Rb, Cs, and B is Ca.

[0028] The Na-doped carbon-coated sodium iron pyrophosphate provided by the present invention is in-situ doped at the Na position to introduce pillar ions, thereby expanding the Na + The diffusion channel is opened, and the cycle stability is improved, which has a positive impact on the electrochemical properties of the material, making it have excellent electrochemical properties, effectively improving the rate performance and cycle stability of the material, and becoming a potential positive electrode material for sodium ion batteries.

[0029] Furthermore, the present invention provides a performance test experiment of Na-doped carbon-coated sodium iron pyrophosphate. It verifies that the three-step heat treatment can stabilize the crystal structure, reduce structural stress, and enhance structural reversibility; it verifies that in-situ doping at the Na position introduces pillar ions and expands the Na + The diffusion channel of the material is opened, and the cycle stability is improved, which has a positive impact on the electrochemical properties of the material, making it have excellent electrochemical properties and effectively improving the rate performance and cycle stability of the material; and it is verified that the introduction of the carbon source can play a chelating role, fully coordinate the complex metal ions, make the material particle size more uniform, and have the effect of reducing trivalent iron and enhancing the electronic conductivity of the material, thereby improving the electronic conductivity of the material.

[0030] Furthermore, the present invention provides a physical and chemical property test experiment of Na-doped carbon-coated sodium ferric pyrophosphate. It verifies that the preparation method provided by the present invention can prepare pure phase and high crystallinity K-doped carbon-coated sodium ferric pyrophosphate positive electrode material; and the experimental process parameters provided by the present invention are suitable, and K-doped carbon-coated sodium ferric pyrophosphate positive electrode material with suitable size and concentrated distribution can be synthesized.

[0031] Furthermore, the present invention verifies that Na-doped carbon-coated sodium iron pyrophosphate has high rate performance and cycle stability.

[0032] The technical solution of the present invention will be further described below in conjunction with specific embodiments.

[0033] Example 1

[0034] This embodiment provides a preparation experiment of Na-doped carbon-coated sodium iron pyrophosphate.

[0035] Take 3.88mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, 0.12mmol potassium dihydrogen phosphate, and 26.5mmol citric acid and dissolve them in deionized water and stir for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 300℃ at a heating rate of 5℃ / min and kept warm for 6h for pre-sintering; grind; heat the furnace body to 300℃ at a heating rate of 5℃ / min and keep warm for 3h; then heat the furnace body to 550℃ at a heating rate of 5℃ / min and keep warm for 8h for sintering, and then cool down to room temperature with the furnace to obtain product Ⅰ (K 0.12 Na 3.88 Fe3(PO4)2P2O7 / C).

[0036] Take 3.85mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, 0.15mmol potassium dihydrogen phosphate, and 26.5mmol citric acid and dissolve them in deionized water, stirring for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 200℃ at a heating rate of 5℃ / min, and kept warm for 6h for pre-sintering; grind; heat the furnace body to 300℃ at a heating rate of 5℃ / min, and keep warm for 3h; then heat the furnace body to 550℃ at a heating rate of 5℃ / min and keep warm for 8h for sintering, and then cool down to room temperature with the furnace to obtain product II (K 0.15 Na 3.85 Fe3(PO4)2P2O7 / C).

[0037] Take 3.88mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, 0.06mmol potassium carbonate, and 26.5mmol citric acid and dissolve them in deionized water, stirring for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 400℃ at a heating rate of 5℃ / min, and kept warm for 6h for pre-sintering; grind; heat the furnace body to 300℃ at a heating rate of 5℃ / min, and keep warm for 3h; then heat the furnace body to 550℃ at a heating rate of 5℃ / min and keep warm for 8h for sintering, and then cool down to room temperature with the furnace to obtain product III (K 0.12 Na 3.88 Fe3(PO4)2P2O7 / C).

[0038] Take 4mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, 0.03mmol lithium carbonate, 0.06mmol potassium dihydrogen phosphate, 26.5mmol citric acid and dissolve in deionized water, stirring for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 300℃ at a heating rate of 5℃ / min, and kept warm for 6h for pre-sintering; grinding; heating to 200℃ at a heating rate of 5℃ / min in the furnace body, and keeping warm for 3h; then heating to 550℃ at a heating rate of 5℃ / min and keeping warm for 8h for sintering, and then cooling down to room temperature with the furnace to obtain product IV (Li 0.06 K 0.06 Na 3.88 Fe3(PO4)2P2O7 / C).

[0039] Take 4mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, 0.06mmol calcium acetate, 26.5mmol citric acid and dissolve them in deionized water, stirring for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 300℃ at a heating rate of 5℃ / min, and kept warm for 6h for pre-sintering; grinding; heating to 400℃ at a heating rate of 5℃ / min in the furnace body, and keeping warm for 3h; then heating to 550℃ at a heating rate of 5℃ / min and keeping warm for 8h for sintering, and then cooling down to room temperature with the furnace to obtain product V (Ca 0.06 Na 3.88 Fe3(PO4)2P2O7 / C).

[0040] Take 3.88mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, 0.12mmol potassium dihydrogen phosphate, and 26.5mmol citric acid and dissolve them in deionized water and stir for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 300℃ at a heating rate of 5℃ / min and kept warm for 6h for pre-sintering; grind; heat the furnace body to 300℃ at a heating rate of 5℃ / min and keep warm for 3h; then heat the furnace body to 400℃ at a heating rate of 5℃ / min and keep warm for 8h for sintering, and then cool down to room temperature with the furnace to obtain product VI (K 0.12 Na 3.88 Fe3(PO4)2P2O7 / C).

[0041] Take 3.88mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, 0.12mmol potassium dihydrogen phosphate, and 26.5mmol citric acid and dissolve them in deionized water and stir for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 300℃ at a heating rate of 5℃ / min and kept warm for 6h for pre-sintering; grind; heat the furnace body to 300℃ at a heating rate of 5℃ / min and keep warm for 3h; then heat the furnace body to 800℃ at a heating rate of 5℃ / min and keep warm for 8h for sintering, and then cool down to room temperature with the furnace to obtain product VII (K 0.12 Na 3.88 Fe3(PO4)2P2O7 / C).

[0042] Take 3.88mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, 0.12mmol potassium dihydrogen phosphate, and 26.5mmol citric acid and dissolve them in deionized water and stir for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 300℃ at a heating rate of 5℃ / min and kept warm for 6h for pre-sintering; grind; heat the furnace body to 550℃ at a heating rate of 5℃ / min and keep warm for 8h for sintering, and then cool down to room temperature with the furnace to obtain product VIII (K 0.12 Na 3.88 Fe3(PO4)2P2O7 / C).

[0043] Take 3.88mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, 0.12mmol potassium dihydrogen phosphate, and 26.5mmol citric acid and dissolve them in deionized water and stir for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 300℃ at a heating rate of 5℃ / min and kept warm for 9h; then the temperature is raised to 550℃ at a heating rate of 5℃ / min and kept warm for 8h for sintering, and then cooled to room temperature with the furnace to obtain product Ⅸ (K 0.12 Na 3.88 Fe3(PO4)2P2O7 / C).

[0044] Take 4mmol sodium dihydrogen phosphate, 3mmol iron nitrate nonahydrate, 0.12mmol potassium dihydrogen phosphate, 26.5mmol citric acid and dissolve them in deionized water, stirring for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 550℃ at a heating rate of 10℃ / min, kept at this temperature for 8h, sintered, and then cooled to room temperature with the furnace to obtain product X(K 0.12 Na 3.88 Fe3(PO4)2P2O7 / C).

[0045] Take 3.88mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, 0.12mmol copper nitrate, and 26.5mmol citric acid and dissolve them in deionized water and stir for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 300℃ at a heating rate of 5℃ / min, and kept warm for 6h for pre-sintering; grind; heat the furnace body to 300℃ at a heating rate of 5℃ / min, and keep warm for 3h; then heat the furnace body to 550℃ at a heating rate of 5℃ / min and keep warm for 8h for sintering, and then cool down to room temperature with the furnace to obtain product Ⅺ (Cu 0.12 Na 3.88 Fe3(PO4)2P2O7 / C).

[0046] Take 4mmol sodium dihydrogen phosphate, 3mmol ferric nitrate nonahydrate, and 26.4mmol citric acid and dissolve them in deionized water, stirring for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 300℃ at a heating rate of 5℃ / min, and kept warm for 6h for pre-sintering; grinding; heating to 300℃ at a heating rate of 5℃ / min in the furnace body, and keeping warm for 3h; then heating to 550℃ at a heating rate of 5℃ / min and keeping warm for 8h for sintering, and then cooling down to room temperature with the furnace to obtain product Ⅻ (Na4Fe3(PO4)2P2O7 / C).

[0047] Take 4mmol sodium dihydrogen phosphate and 3mmol ferric nitrate nonahydrate and dissolve them in deionized water, stir for 2h. Spray drying is performed at an inlet temperature of 260℃ and a feed rate of 800mL / h. Argon is introduced into a tubular furnace, and the furnace body is heated to 300℃ at a heating rate of 5℃ / min, and kept warm for 6h for pre-sintering; grind; heat the furnace body to 300℃ at a heating rate of 5℃ / min, and keep warm for 3h; then heat the furnace body to 550℃ at a heating rate of 5℃ / min and keep warm for 8h for sintering, and then cool down to room temperature with the furnace to obtain product ⅩⅢ (Na4Fe3(PO4)2P2O7).

[0048] Example 2

[0049] This embodiment provides a performance test experiment of Na-doped carbon-coated sodium iron pyrophosphate. 0.7g of product I, 0.2g of conductive agent (acetylene black is used in this experiment) and 0.1g of binder (polyvinylidene fluoride, PVDF is used in this experiment) are mixed in 1g of polar solvent (N-methylpyrrolidone, NMP is used in this experiment) to obtain positive electrode slurry I; the obtained positive electrode slurry I is coated on the positive electrode current collector of the battery (aluminum foil is used in this experiment), and dried at 90°C in a vacuum drying oven for 10 hours to obtain the positive electrode sheet matrix I. The obtained positive electrode sheet matrix I was cut into a circle with a diameter of 12 mm and used as the positive electrode sheet I, and assembled with other parts into a button battery I, wherein the electrolyte in the assembled button battery I was a 1 mol / L sodium salt solution, the solute of which was NaClO4, and the solvent was ethylene carbonate (EC) and ethylene methyl carbonate (EMC) in a volume ratio of 1:1, and 5% fluoroethylene carbonate (FEC) additive was additionally added to the electrolyte.

[0050] The same amount of products II to XIII were used to replace product I, respectively, to obtain button batteries II to XIII; the electrochemical properties of products I to XIII were tested using assembled button batteries I to XIII as carriers, wherein the test current 1C was 129 mA / g, and the charge and discharge temperature was room temperature 25°C. The test results are shown in Table 1.

[0051] Table 1 Electrochemical properties of products Ⅰ to IX

[0052] Test product Chemical formula 0.1C Gram Capacity 1C Gram Capacity Product I <h2 style=";text-align:left;direction:ltr"><![CDATA[K <h2 style=";text-align:left;direction:ltr"> 0.12 <h2 style=";text-align:left;direction:ltr"> Na<h2 style=";text-align:left;direction:ltr"> 3.88 <h2 style=";text-align:left;direction:ltr"> Fe3(PO4)2P2O7 / C]]><h2 style=";text-align:left;direction:ltr"> 128mAh / g 114mAh / g Product II <h2 style=";text-align:left;direction:ltr"><![CDATA[K <h2 style=";text-align:left;direction:ltr"> 0.15 <h2 style=";text-align:left;direction:ltr"> Na<h2 style=";text-align:left;direction:ltr"> 3.85 <h2 style=";text-align:left;direction:ltr"> Fe3(PO4)2P2O7 / C]]><h2 style=";text-align:left;direction:ltr"> 117mAh / g 101mAh / g Product III <h2 style=";text-align:left;direction:ltr"><![CDATA[Li <h2 style=";text-align:left;direction:ltr"> 0.12 <h2 style=";text-align:left;direction:ltr"> Na<h2 style=";text-align:left;direction:ltr"> 3.88 <h2 style=";text-align:left;direction:ltr"> Fe3(PO4)2P2O7 / C]]><h2 style=";text-align:left;direction:ltr"> 114mAh / g 97mAh / g Product IV <![CDATA[Li 0.06 K 0.06 Na 3.88 Fe3(PO4)2P2O7 / C]]> 105mAh / g 99mAh / g Product V <h2 style=";text-align:left;direction:ltr"><![CDATA[Ca <h2 style=";text-align:left;direction:ltr"> 0.06 <h2 style=";text-align:left;direction:ltr"> Na<h2 style=";text-align:left;direction:ltr"> 3.88 <h2 style=";text-align:left;direction:ltr"> Fe3(PO4)2P2O7 / C]]><h2 style=";text-align:left;direction:ltr"> 105mAh / g 98mAh / g Product VI <h2 style=";text-align:left;direction:ltr"><![CDATA[K <h2 style=";text-align:left;direction:ltr"> 0.12 <h2 style=";text-align:left;direction:ltr"> Na<h2 style=";text-align:left;direction:ltr"> 3.88 <h2 style=";text-align:left;direction:ltr"> Fe3(PO4)2P2O7 / C]]><h2 style=";text-align:left;direction:ltr"> 51mAh / g 38mAh / g Product VII <h2 style=";text-align:left;direction:ltr"><![CDATA[K <h2 style=";text-align:left;direction:ltr"> 0.12 <h2 style=";text-align:left;direction:ltr"> Na<h2 style=";text-align:left;direction:ltr"> 3.88 <h2 style=";text-align:left;direction:ltr"> Fe3(PO4)2P2O7 / C]]><h2 style=";text-align:left;direction:ltr"> 42mAh / g 31mAh / g Product VIII <h2 style=";text-align:left;direction:ltr"><![CDATA[K <h2 style=";text-align:left;direction:ltr"> 0.12 <h2 style=";text-align:left;direction:ltr"> Na<h2 style=";text-align:left;direction:ltr"> 3.88 <h2 style=";text-align:left;direction:ltr"> Fe3(PO4)2P2O7 / C]]><h2 style=";text-align:left;direction:ltr"> 92mAh / g 81mAh / g Product IX <h2 style=";text-align:left;direction:ltr"><![CDATA[K <h2 style=";text-align:left;direction:ltr"> 0.12 <h2 style=";text-align:left;direction:ltr"> Na<h2 style=";text-align:left;direction:ltr"> 3.88 <h2 style=";text-align:left;direction:ltr"> Fe3(PO4)2P2O7 / C]]><h2 style=";text-align:left;direction:ltr"> 99mAh / g 83mAh / g Product X <h2 style=";text-align:left;direction:ltr"><![CDATA[K <h2 style=";text-align:left;direction:ltr"> 0.12 <h2 style=";text-align:left;direction:ltr"> Na<h2 style=";text-align:left;direction:ltr"> 3.88 <h2 style=";text-align:left;direction:ltr"> Fe3(PO4)2P2O7 / C]]><h2 style=";text-align:left;direction:ltr"> 91mAh / g 72mAh / g Product Ⅺ <h2 style=";text-align:left;direction:ltr"><![CDATA[Cu <h2 style=";text-align:left;direction:ltr"> 0.12 <h2 style=";text-align:left;direction:ltr"> Na<h2 style=";text-align:left;direction:ltr"> 3.88 <h2 style=";text-align:left;direction:ltr"> Fe3(PO4)2P2O7 / C]]><h2 style=";text-align:left;direction:ltr"> 60mAh / g 53mAh / g Product Ⅻ <![CDATA[Na4Fe3(PO4)2P2O7 / C]]> 96mAh / g 84mAh / g Product XIII <![CDATA[Na4Fe3(PO4)2P2O7]]> 51mAh / g 41mAh / g

[0053] It can be seen from Table 1 that products Ⅰ to Ⅴ have better capacities, among which product Ⅰ and product Ⅱ have the best capacities.

[0054] Compared with product I, product VIII did not undergo the first stage of sintering, which resulted in uneven material particle size, making sintering and agglomeration likely to occur during the subsequent calcination process. In addition, its structure was not stable enough, which had a certain impact on the discharge capacity and cycle performance.

[0055] Compared with product I, product IX did not undergo the grinding step between pre-calcination and sintering, resulting in uneven distribution of particles in the material, easy sintering and agglomeration, and easily causing an increase in internal resistance, which has an adverse effect on the discharge capacity and cycle stability performance.

[0056] The three-step heat treatment can stabilize the crystal structure, reduce structural stress, and enhance structural reversibility. Compared with product I, product X did not undergo the three-step heat treatment, and the material failed to form a good nucleation, resulting in large differences in the morphology specifications of the material, which had a certain impact on the performance.

[0057] Compared with product I, the introduced Cu element in product XI partially fails to enter the Na site and becomes an impurity. Excessive impurity elements lead to an unstable crystal structure and have a certain impact on the performance of the material.

[0058] Compared with product I and product II, product XII did not introduce other doping elements at the Na site, and failed to have pillar ions to support the material structure to expand the diffusion channel of Na and improve the cycle stability, resulting in poor Na diffusion kinetics, poor material cycle stability, and structural collapse after long-term cycling.

[0059] Compared with product I and product II, product XIII did not introduce citric acid and other carbon sources to play a chelating role, and failed to fully coordinate the complex metal ions, resulting in the inability to smoothly synthesize the material and large differences in the particle size of the material. In addition, it failed to reduce trivalent iron and enhance the electronic conductivity of the material, resulting in extremely low electronic conductivity of the material.

[0060] Example 3

[0061] This embodiment provides a physical and chemical property test experiment of Na-doped carbon-coated sodium iron pyrophosphate.

[0062] The product I prepared in Example 1 was subjected to X-ray diffraction test (XRD) using the Rigaku Smart Lab. The radiation source used in XRD was a copper target, the tube voltage was 40 kV, the tube current was 200 mA, the scanning step was 0.01, the scanning angle range was 5° to 65°, the scanning speed was 8° / min, and the XRD spectrum was as follows: Figure 1 As shown. Figure 1 It can be seen from the XRD spectrum of product Ⅰ (K 0.12 Na 3.88 Fe3(PO4)2P2O7 / C) has a pure phase crystal structure of Pn21a space group with high crystallinity (PDF standard card number: PDF#89-0579). No obvious impurity diffraction peaks were observed, indicating that the addition of a small amount of K element did not affect the crystal structure of the material. This result shows that the experimental method for preparing product I in Example 1 can prepare a pure phase and highly crystallinity K-doped carbon-coated sodium iron pyrophosphate positive electrode material.

[0063] The product I prepared in Example 1 was observed by scanning electron microscope (FlexSEM1000Ⅱ), and the image was as follows: Figure 2 As shown. Figure 2 It can be seen that the primary particles of the obtained material are relatively uniform and spherical. The particle size is between 50 and 500 nm. Among them, due to the presence of the carbon source, the primary particles agglomerated a little, and the secondary particles after agglomeration are generally less than 3 microns. This shows that the experimental process parameters are suitable and can synthesize K-doped carbon-coated sodium iron pyrophosphate positive electrode materials with small size and concentrated distribution.

[0064] The button cell I, button cell XII and button cell XIII prepared in Example 2 were subjected to 5 charge-discharge cycles at 0.1C, 0.3C, 0.5C, 1C, 2C, 5C and 0.1C rates respectively at 25°C and in the voltage range of 1.8-4.2V. After each charge-discharge cycle, they were left standing for 1 minute to test the rate performance of button cell I, button cell XII and button cell XIII. The results are as follows: Figure 3 The discharge capacity results shown are Figure 4 The charge and discharge curves shown are Figure 3 and Figure 4 It can be seen that the 0.1C first-cycle discharge specific capacity of button battery I is 128mAh / g, and the 5C first-cycle capacity is 114mAh / g, which maintains 89.1% of the initial capacity; the 0.1C first-cycle discharge specific capacity of button battery XII is 92.9mAh / g, and the 5C first-cycle capacity is 70.36mAh / g, which maintains 75.7% of the initial capacity; the 0.1C first-cycle discharge specific capacity of button battery XIII is 49.3mAh / g, and the 5C first-cycle capacity is 32.2mAh / g, which maintains 62.9% of the initial capacity.

[0065] The button cell I, button cell XII and button cell XIII prepared in Example 2 were subjected to charge and discharge tests respectively, with a current of 1C of 129 mA / g and a charge and discharge temperature of 25° C. as room temperature. Figure 5 The cycle performance curve shown is Figure 5 It can be seen that within the voltage range of 1.8 to 4.2 V and at a rate of 1C, the first charge and discharge capacity of button battery I is 114.4 mAh / g, and after 200 cycles, the capacity retention rate is 97.3%; the first charge and discharge capacity of button battery XII is 98.5 mAh / g, and after 200 cycles, the capacity retention rate is 86.3%; the first charge and discharge capacity of button battery XIII is 45.1 mAh / g, and after 200 cycles, the capacity retention rate is 70.1%.

[0066] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0067] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A Na-doped carbon-coated sodium iron pyrophosphate, It is characterized in that Its chemical formula is A x B y Na 4-x-2y Fe 3 (PO 4 ) 2 P 2 O 7 / C; Among them, 0≤x≤0.2, 0≤y≤0.2, and x+2y>0, A is one or a combination of Li, K, Rb, Cs, and B is Ca.

2. The Na-doped carbon-coated sodium iron pyrophosphate according to claim 1, It is characterized in that The particle size of the Na-doped carbon-coated sodium iron pyrophosphate is 20 nm to 10 μm.

3. A method for preparing the Na-doped carbon-coated sodium ferric pyrophosphate according to any one of claims 1 to 2, It is characterized in that The following steps are involved: Mixing and dissolving the A source / B source, the sodium source, the iron source, the phosphorus source and the carbon source in water, and sequentially drying and grinding the obtained mixed solution to obtain a precursor; The precursor is sequentially pre-fired at 200-400° C. in an inert atmosphere, secondary ground, and sintered in two stages in an inert atmosphere to obtain the Na-doped carbon-coated sodium iron pyrophosphate; wherein, in the two stages, the temperature condition of the first stage is 200-400° C., and the temperature condition of the second stage is 500-700° C.

4. The preparation method according to claim 3, It is characterized in that The A source is one or a combination of dihydrogen phosphate A, bicarbonate A, sulfuric acid A, chloric acid A, carbonate A, acetic acid A, and fluoride A; the B source is one or a combination of dihydrogen phosphate B, bicarbonate B, sulfuric acid B, chloric acid B, carbonate B, acetic acid B, and fluoride B; And / or, the sodium source is one or a combination of sodium dihydrogen phosphate and disodium hydrogen phosphate; And / or, the iron source is one or a combination of ferrous nitrate, ferrous acetate, ferrous oxalate and ferrous sulfate; And / or, the carbon source is one or a combination of citric acid, vitamin C, glucose and oxalic acid.

5. The preparation method according to claim 3, It is characterized in that The molar ratio of the A source / B source, the sodium source and the iron source is the molar ratio of each element in the chemical formula; And / or, the ratio of the mass of the carbon source to the sum of the masses of the A source / B source, the sodium source, the iron source and the phosphorus source is 1:2-4.

6. The preparation method according to claim 3, It is characterized in that The mixed solution is stirred in water for 1 to 4 hours; And / or, the drying method is spray drying or freeze drying, and the drying conditions are: inlet temperature 200-300° C., feed rate 500-1000 mL / h; And / or, the inert atmosphere is one or a combination of nitrogen, argon and hydrogen; And / or, the pre-calcination temperature rise rate is 1-10°C / min, and the heat preservation time is 0.5-6h; And / or, the heating rate of the first stage is 0.5-10°C / min, and the insulation time is 2-5h, and the heating rate of the second stage is 0.5-10°C / min, and the insulation time is 4-10h.

7. Use of the Na-doped carbon-coated sodium ferric pyrophosphate according to any one of claims 1 to 2 or the Na-doped carbon-coated sodium ferric pyrophosphate prepared by the preparation method according to any one of claims 3 to 6 in the preparation of positive electrode materials for sodium ion batteries.

8. A sodium ion battery cathode material, It is characterized in that The invention comprises a conductive agent, a binder and an active material, wherein the active material comprises the Na-doped carbon-coated sodium ferric pyrophosphate according to any one of claims 1 to 2 or the Na-doped carbon-coated sodium ferric pyrophosphate prepared by the preparation method according to any one of claims 3 to 6.

9. A method for preparing the positive electrode material for a sodium ion battery according to claim 8, It is characterized in that The following steps are involved: Dissolving the Na-doped carbon-coated sodium iron pyrophosphate, a conductive agent and a binder in a polar solvent at a mass ratio of 7 to 8:1 to 2:1; The positive electrode material is applied on the positive electrode current collector of the battery and dried to obtain the positive electrode material of the Na ion battery.

10. The preparation method according to claim 9, It is characterized in that The conductive agent is acetylene black; And / or, the binder is polyvinylidene fluoride; and / or, the polar solvent N-methylpyrrolidone; and / or, the mass ratio of the Na-doped carbon-coated sodium iron pyrophosphate, the conductive agent and the binder is 7:2:1; And / or, the battery positive electrode current collector is aluminum foil; And / or, the drying condition is 90° C. and 10 h.

Citation Information

Patent Citations

  • Positive electrode material, positive plate and sodium ion battery

    CN117080393A

  • Carbon-coated lithium iron phosphate-sodium ferric phosphate pyrophosphate positive electrode material, preparation method, positive electrode plate and lithium ion battery

    CN118263421A

  • Iron-based sodium ion full battery and preparation method therefor

    WO2024011862A1

Cited By

  • Pyrophosphate ferric sodium phosphate / C composite material and preparation and application thereof in sodium ion battery

    CN120057883A

  • In-situ doped composite sodium iron phosphate positive material, preparation method thereof and sodium ion battery

    CN120288732B

  • Modified ferric sodium pyrophosphate positive electrode material as well as preparation method and application thereof

    CN121366889A