Fuel cell catalyst carbon carrier and preparation method thereof

Through a step-by-step calcination method of zinc citrate and polymer materials, a carbon support with high specific surface area and hierarchical pore structure is prepared, which solves the problems of agglomeration and activity reduction of platinum particles in fuel cell catalysts, and improves the performance and performance of the catalyst. Process efficiency.

CN118851146APending Publication Date: 2024-10-29CHINA AUTOMOTIVE INNOVATION CORP

Patent Information

Application Number
CN202410857480.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing fuel cell catalyst carbon carriers have problems such as agglomeration of platinum particles, large particle size, and easy coating by resin, resulting in reduced activity. Moreover, the preparation method of high specific surface area and multi-level pore structure is complex and costly, which cannot meet the performance requirements of fuel cells. .

Method used

Zinc citrate is used as a self-template to combine with polymer materials, and a carbon support with high specific surface area and hierarchical pore structure is prepared through one-step step-by-step high-temperature calcination, which avoids the template introduction and removal steps and simplifies the process flow.

Benefits of technology

The carbon carrier with high specific surface area and hierarchical pore structure is realized, which improves the activity and material transfer efficiency of the fuel cell catalyst, and reduces the preparation cost and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851146A_ABST
    Figure CN118851146A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fuel cell catalysts, in particular to a fuel cell catalyst carbon carrier and a preparation method thereof. The preparation method of the fuel cell catalyst carbon carrier comprises the following steps: taking zinc citrate and a high polymer material as raw materials, and carrying out stepped high-temperature calcination to obtain the fuel cell catalyst carbon carrier, the high polymer material is selected from one or more of polyacrylonitrile, polypyrrole, polyvinylpyrrolidone, polyaniline and polydopamine. The porous carbon carrier with high specific surface area and rich porosity is directly prepared by simply calcining multiple precursor carbon sources in a one-step stepped manner, and the pore distribution and the specific surface area range can be effectively adjusted by selecting zinc citrate and a high-molecular carbon source; the requirements of the platinum-carbon catalyst carbon carrier meeting the working conditions of a fuel cell are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fuel cell catalysts, and in particular to a fuel cell catalyst carbon carrier with high specific surface area and multi-level pore distribution and a preparation method thereof. Background Art

[0002] Hydrogen energy is a low-carbon, clean, zero-emission energy carrier. Its high calorific value and clean renewable characteristics will play a vital role in replacing traditional fossil energy, achieving carbon peak and carbon neutrality goals and energy security. Fuel cells, as a key energy conversion device in the hydrogen energy industry, can effectively convert the chemical energy in hydrogen energy into electrical energy and release it. Efficient fuel cell devices are essential for promoting energy conservation and emission reduction and the development of a hydrogen-electric society. The energy conversion efficiency of fuel cells is mainly limited by the activity and stability of the fuel cell catalyst, especially at the cathode of the fuel cell. The electrocatalytic oxygen reduction reaction of the cathode catalyst, which has slower kinetics, has become the key to determining the performance of the fuel cell.

[0003] The cathode oxygen reduction catalyst of fuel cells is mainly a platinum-carbon catalyst, which is mainly composed of a carbon carrier and platinum nanoparticles loaded thereon. The active center is the platinum nanoparticle, but the activity of the platinum particles is often more dependent on the good conductivity, mass transfer, anchoring and stabilization of the platinum particles by the carbon carrier. The development of excellent catalyst carbon carrier materials is crucial to achieving high-performance fuel cell performance. However, at this stage, platinum-carbon catalysts often face problems such as platinum particle agglomeration, large particle size, and easy poisoning by resin coating in the membrane electrode, which reduces activity. Therefore, it is urgent to develop catalyst carbon carriers with high specific surface area and rich pore structure to solve the above problems, and to develop simple, low-cost and efficient carrier synthesis methods to promote the development of fuel cell catalysts.

[0004] The synthesis of high specific surface area and multi-level porous carbon materials mostly relies on chemical etching or template preparation, which generally uses corrosive strong alkali, strong acid, carbon dioxide and other gases, but has limited ability to control the pore structure, and is not easy to form a multi-level porous structure of micropores, mesopores and macropores at the same time. The steps are cumbersome, the equipment requirements are high and the energy consumption is high. The template method involves the introduction and removal of the template, and the specific surface area is often not high enough, which also leads to a more complicated preparation process and higher costs. Both methods are temporarily unable to meet the development needs of fuel cell catalyst carbon carriers. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a fuel cell catalyst carbon support and a preparation method thereof. The preparation method provided by the present invention uses low-cost zinc citrate as a self-template and combines a polymer material as a carbon source, and directly prepares a carbon support with a high specific surface area and a hierarchical pore structure through a one-step high-temperature calcination without the need for post-processing to remove the template and activation steps. The carbon support has the characteristics of being highly adjustable and is suitable for a fuel cell platinum-carbon catalyst carbon support material.

[0006] In a first aspect, the present invention provides a method for preparing a fuel cell catalyst carbon carrier, comprising: using zinc citrate and a polymer material as raw materials, and obtaining a fuel cell catalyst carbon carrier by step-by-step high-temperature calcination; the polymer material is selected from one or more of polyacrylonitrile, polyvinyl pyrrolidone, polyaniline, and polydopamine.

[0007] The present invention uses zinc citrate as a precursor and a pore-forming agent, and through step-type temperature control, oxides are formed at low temperature to form mesopores and macropores, and then zinc oxide is volatilized at high temperature to form micropores, and then a specific polymer carbon source is introduced to further adjust the pore distribution and specific surface area range. In the process of zinc citrate gradient heating, as the temperature gradually rises, larger zinc oxide nanoparticles surrounded by carbon carriers are first generated, and the zinc oxide particles are gradually grown at a low temperature and constant temperature for a period of time, and then they are reduced to zinc element at a high temperature and constant temperature, and finally evaporated, and the particles disappear, and micropores and mesopores are introduced at the same time, and the pore distribution and specific surface area range are adjusted in combination with specific polymer materials, which can better meet the needs of fuel cell catalysts.

[0008] More preferably, the polymer material is polydopamine, polyvinyl pyrrolidone or polypyrrole, preferably polydopamine.

[0009] The present invention has found that when the above-mentioned polydopamine polymer material is used, a larger amount of microporous carbon structure can be produced after high-temperature decomposition, and a large amount of nitrogen doping can be achieved. In combination with zinc citrate, an excellent mesoporous structure can be produced during the step-by-step calcination process, thereby better realizing a hierarchical pore structure, which has an unexpected effect on accelerating material transfer in the actual application of fuel cells.

[0010] Preferably, the mass ratio of the zinc citrate to the polymer carbon source is 0.1:1 to 3:1.

[0011] More preferably, the mass ratio of the zinc citrate to the polymer carbon source is 0.5:1 to 3:1, preferably 0.6:1 to 1:1. For example, the mass ratio of zinc citrate to the polymer carbon source can be 0.5:1, 0.6:1, 1:1, 2:1, 3:1, etc.

[0012] Preferably, the stepped high-temperature calcination includes: the stepped high-temperature calcination includes: heating to 600-700°C at a first heating rate, keeping warm for 1-4 hours, then heating to 800-1200°C at a second cooling rate, keeping warm for 1-4 hours, and then cooling to 300-350°C at a second cooling rate.

[0013] Further preferably, the first heating rate and the second heating rate are each 2-20°C / min; and / or the second heating rate is 2-20°C / min; and / or the cooling rate is 2-10°C / min.

[0014] In the present invention, by adopting the above-mentioned precursor carbon source and self-templated zinc citrate, in combination with a specific programmed temperature rising method, a microporous-mesoporous porous carbon structure is successfully constructed, which has a high specific surface area and a hierarchical structure, and can give full play to the activity of the platinum-carbon catalyst and its material transport characteristics for practical application in fuel cells.

[0015] Preferably, the method further comprises grinding the zinc citrate and the polymer material, wherein the grinding time is 10 to 30 minutes, for example, the grinding time may be 10 minutes, 15 minutes, 20 minutes, 25 minutes, or 30 minutes.

[0016] Preferably, the high-temperature calcination is carried out under an inert atmosphere; preferably, it includes introducing nitrogen to provide an inert nitrogen atmosphere, and the gas flow rate is preferably 30 to 200 cc / min.

[0017] Further preferably, the zinc citrate and polydopamine are ground for 10 to 30 minutes; then the ground mixture is heated stepwise under an inert atmosphere, with an inert gas flow rate of 30 to 200 cc / min and a heating rate of 2 to 20°C / min, first heated to 600 to 650°C, kept warm for 1 to 4 hours, then heated to 800 to 1200°C, kept warm for 1 to 4 hours; then programmed cooling, with a cooling rate of 2 to 10°C / min, cooled to 300 to 350°C, and then cooled naturally.

[0018] The preparation method of the fuel cell platinum-carbon catalyst carbon carrier provided by the present invention has the advantages of simple preparation process, easy to obtain raw materials, low equipment and process requirements, etc., and compared with the traditional activation method which is difficult to construct a mesoporous structure and the template method which is difficult to obtain a high specific surface area carbon carrier, the present invention can directly prepare a porous carbon carrier with high specific surface area and rich porosity by simply calcining a variety of precursor carbon sources in a one-step manner, and the pore size and specific surface area range can be more effectively adjusted by selecting a polymer carbon source to better meet the requirements of the platinum-carbon catalyst carbon carrier that meets the operating conditions of the fuel cell.

[0019] In a second aspect, the present invention also provides a fuel cell catalyst carbon carrier prepared by the above preparation method.

[0020] In a third aspect, the present invention also provides a fuel cell catalyst carbon carrier prepared by the above preparation method or the use of the above fuel cell catalyst carbon carrier in the preparation of a fuel cell catalyst.

[0021] In a fourth aspect, the present invention further provides a fuel cell catalyst, a fuel cell catalyst carbon carrier prepared by the above-mentioned method for preparing the fuel cell catalyst carbon carrier or the above-mentioned fuel cell catalyst carbon carrier.

[0022] Preferably, the platinum loading of the fuel cell catalyst is 20 wt% to 60 wt%.

[0023] Preferably, the method for preparing the fuel cell catalyst comprises: mixing the fuel cell catalyst carbon carrier with a chloroplatinic acid solution, adding water and performing ice bath ultrasound, then heating and magnetic stirring, freeze drying, and high temperature reduction to obtain a fuel cell catalyst.

[0024] Preferably, the reduction temperature is 150-500° C. and the time is 1-3 hours.

[0025] The present invention adopts a self-template method, and uses simple raw materials, metal organic molecules zinc citrate and polymer materials directly as precursor carbon sources to prepare porous carbon carriers, which has the advantages of simple raw material sources, controllable costs, streamlined synthesis routes, and highly controllable carbon carrier structural characteristics. At present, the preparation of porous carbon with high specific surface area and multi-level pore structure mainly adopts a template method or a method of first preparing a carbon carrier and then chemically etching. The template method for preparing porous carbon carriers often uses silicon dioxide or metal oxides as a template, and then carbonizes the organic precursor at high temperature to prepare the carbon material, and then etches the template with strong alkali or hydrofluoric acid to prepare porous carbon. Not only is the route complicated, but also the template material needs to be customized, and it has the characteristics of high energy consumption and high pollution. The activator method for preparing porous carbon often uses materials such as strong alkali and oxidizing acid, and it is necessary to first prepare the carbon material and then activate it to form pores, which often leads to high energy consumption and high pollution. Therefore, the one-step stepped temperature calcination method of the present invention utilizes a self-template approach to avoid the introduction and removal of templates. At the same time, the introduction of zinc can serve as a pore-forming agent to further enrich the pore structure by introducing mesopores and micropores, thereby increasing the specific surface area. This highly adjustable route provides a very simple, universal and inexpensive route for the precise design of the morphology of porous carbon carriers, greatly improving the design and synthesis efficiency of fuel cell catalyst carbon carriers.

[0026] The beneficial effects of the present invention are at least: 1) The present invention directly uses a simple carbon-containing organic molecule zinc citrate as a precursor, rather than first forming a complex precursor template with a special structure. A porous carbon carrier with a high specific surface area and rich microporous and mesoporous structure can be directly prepared by a one-step temperature calcination method without the need for other post-treatment processes.

[0027] 2) The present invention innovatively uses zinc citrate as a carbon source and pore-forming agent, without the need for other template agents and activator components. At the same time, the present invention adopts a step-by-step temperature calcination method, which can introduce mesopores by generating large particles of zinc oxide during low-temperature calcination, and then reduce it to zinc element at high temperature to introduce additional micropores, ultimately achieving a specific surface area of ​​up to 1770m 2 g -1 The average pore size is close to 5nm, and there are both microporous and mesoporous carbon support materials.

[0028] 3) The present invention can further improve the specific surface area and pore adjustment ability by mixing specific polymer materials (polyacrylonitrile, polypyrrole, polyvinyl pyrrolidone, polyaniline, polydopamine) as binary carbon sources and calcining them with zinc citrate, continuing the advantages of preparing graded porous carbon by a one-step temperature calcination method. In addition, by simply selecting polymers with different molecular weights and component structures, as well as different ratios of zinc citrate and polymer materials, a porous carbon carrier material with a certain specific surface area and pore size distribution suitable for fuel cells can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. It is obvious that the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 This is a scanning electron microscope image of the porous carbon support of Example 1 of the present invention.

[0031] Figure 2 The nitrogen adsorption-desorption isotherm curves for analyzing the specific surface area of ​​the porous carbon carriers of Examples 1-5 of the present invention.

[0032] Figure 3 This is a test diagram of the electrocatalytic oxygen reduction performance of the platinum-carbon catalyst prepared using the porous carbon of Example 1 as a carrier in the present invention.

[0033] Figure 4 This is the specific surface area and pore size distribution diagram of Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] If no specific technology or conditions are specified in the embodiments of the present invention, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the devices, instruments, reagents, etc. is not specified, they are all conventional products that can be purchased through regular channels. The raw materials used in the present invention can be easily purchased in the domestic product market.

[0036] Example 1

[0037] Zinc citrate and polymer carbon source polydopamine are mixed in a certain mass ratio (zinc citrate: polymer carbon source = 0.5:1), and then the precursor zinc citrate and polymer carbon source mixture is ground in an agate mortar for 30 minutes, placed in a corundum crucible, and placed in a tubular furnace, nitrogen is introduced into the tubular furnace to ensure that an inert nitrogen atmosphere is always maintained during the high temperature process, and the gas flow rate is 100cc / min, and then the temperature is programmed to rise at a rate of 5°C / min to a target temperature of 600°C, maintained at the target temperature for 1h, and then programmed to rise to 800°C, maintained at the target temperature for 1h, and the temperature is programmed to rise at a rate of 10°C / min, and then programmed to cool at a rate of 2°C / min to 300°C, and then naturally cooled to room temperature to finally obtain a carbon carrier material.

[0038] The present embodiment also provides a platinum-carbon catalyst, which is prepared by an impregnation method, and the specific steps are as follows: weigh 70 mg of the carbon carrier prepared in the present embodiment and place it in a 50 ml beaker; then measure 1.868 ml of chloroplatinic acid solution, the concentration of which is 0.2 mol, then add 4.5 ml of pure water thereto, and ultrasonicate in an ice bath for 10 min; then continuously perform magnetic stirring to evaporate the solution during heating at 70 ° C until most of the liquid disappears and the whole is viscous and paste-like, and then place it in a freeze dryer for freeze drying overnight; place the dried sample in a crucible, and then reduce it in a tubular furnace in a 10% hydrogen-argon mixed gas, the reduction temperature is 150 ° C, the time is 1 h, and finally obtain a (platinum loading 50wt%) platinum-carbon catalyst. The following examples prepare platinum-carbon catalysts with the same steps.

[0039] Example 2

[0040] This embodiment provides a multi-level pore structure carbon carrier material, and the specific steps are as follows: Zinc citrate and polymer carbon source polyacrylonitrile are mixed in a mass ratio (zinc citrate: polymer carbon source = 0.5:1), and then the precursor zinc citrate and polymer carbon source mixture is ground in an agate mortar for 30 minutes, the mixture is placed in a corundum crucible, and placed in a tubular furnace, nitrogen is introduced into the tubular furnace to ensure that an inert nitrogen atmosphere is always maintained during the high temperature process, the gas flow rate is 100cc / min, and then the temperature is programmed to rise at a rate of 5°C / min to a target temperature of 600°C, maintained at the target temperature for 1h, and then programmed to rise to 800°C, maintained at the target temperature for 1h, the heating rate is 10°C / min, and then programmed to cool at a rate of 2°C / min to 300°C, and then naturally cooled to room temperature to finally obtain a carbon carrier material.

[0041] Example 3

[0042] Zinc citrate and polymer carbon source polypyrrole are mixed in a mass ratio (zinc citrate: polymer carbon source = 0.5:1), and then the precursor zinc citrate and polymer carbon source mixture is ground in an agate mortar for 30 minutes, the mixture is placed in a corundum crucible, and placed in a tubular furnace, nitrogen is introduced into the tubular furnace to ensure that an inert nitrogen atmosphere is always maintained during the high temperature process, the gas flow rate is 100cc / min, and then the temperature is programmed to rise at a rate of 10°C / min to a target temperature of 800°C, maintained at the target temperature for 2h, and then programmed to cool at a rate of 2°C / min to 300°C, and then naturally cooled to room temperature to finally obtain a carbon carrier material.

[0043] Example 4

[0044] Zinc citrate and polymer carbon source polyvinyl pyrrolidone K30 are mixed in a mass ratio (zinc citrate: polymer carbon source = 0.5:1), and then the precursor zinc citrate and polymer carbon source mixture is ground in an agate mortar for 30 minutes, the mixture is placed in a corundum crucible, and placed in a tubular furnace, nitrogen is introduced into the tubular furnace to ensure that an inert nitrogen atmosphere is always maintained during the high temperature process, the gas flow rate is 100cc / min, and then the temperature is programmed to rise at a rate of 5°C / min to a target temperature of 600°C, maintained at the target temperature for 1h, and then programmed to rise to 800°C at a rate of 10°C / min, and then programmed to cool at a rate of 2°C / min to 300°C, and then naturally cooled to room temperature to finally obtain a carbon carrier material.

[0045] Example 5

[0046] Zinc citrate and polymer carbon source polyvinyl pyrrolidone K88 are mixed in a mass ratio (zinc citrate: polymer carbon source = 0.5:1), and then the precursor zinc citrate and polymer carbon source mixture is ground in an agate mortar for 30 minutes, the mixture is placed in a corundum crucible, and placed in a tubular furnace, nitrogen is introduced into the tubular furnace to ensure that an inert nitrogen atmosphere is always maintained during the high temperature process, the gas flow rate is 100cc / min, and then the temperature is programmed to rise at a rate of 5°C / min to a target temperature of 600°C, maintained at the target temperature for 1h, and then programmed to rise to 800°C at a rate of 10°C / min, and then programmed to cool at a rate of 2°C / min to 300°C, and then naturally cooled to room temperature to finally obtain a carbon carrier material.

[0047] Example 6

[0048] Zinc citrate and polymer carbon source polyaniline are mixed in a mass ratio, such as zinc citrate: polymer carbon source = 0.5:1, and then the precursor zinc citrate and polymer carbon source mixture is ground in an agate mortar for 30 minutes, and the mixture is placed in a corundum crucible and placed in a tubular furnace. Nitrogen is introduced into the tubular furnace to ensure that an inert nitrogen atmosphere is always maintained during the high temperature process. The gas flow rate is 100cc / min, and then the temperature is programmed to rise at a rate of 5℃ / min to a target temperature of 600℃, maintained at the target temperature for 1h, and then programmed to rise to 800℃ at a rate of 10℃ / min, and then programmed to cool at a rate of 2℃ / min to 300℃, and then naturally cooled to room temperature to finally obtain a carbon carrier material. Its specific surface area is 852m 2 g -1 , the average pore size is 3.5nm.

[0049] Example 7

[0050] Zinc citrate and polymer carbon source polydopamine were mixed in a mass ratio (zinc citrate: polymer carbon source = 1:1), and then the precursor zinc citrate and polymer carbon source mixture was ground in an agate mortar for 30 minutes, and the mixture was placed in a corundum crucible and placed in a tube furnace. Nitrogen was introduced into the tube furnace to ensure that an inert nitrogen atmosphere was always maintained during the high temperature process. The gas flow rate was 100cc / min, and then the temperature was programmed to rise at a rate of 5℃ / min to a target temperature of 600℃, maintained at the target temperature for 1h, and then programmed to rise to 800℃ at a rate of 10℃ / min, and then programmed to cool at a rate of 2℃ / min to 300℃, and then naturally cooled to room temperature to finally obtain a carbon carrier material. Its specific surface area is 1257m 2 g -1, and its average pore size is 4.8nm.

[0051] Example 8

[0052] The same method as in Example 1 was used, except that the mass ratio of zinc citrate to the polymer carbon source was 0.1:1. Its specific surface area was 1257 m 2 g -1 , and its average pore size is 4.8nm.

[0053] Comparative Example 1

[0054] The zinc citrate precursor 6g was heated to 800℃ at 5℃ / min and kept at this temperature for 2h, and finally cooled to 300℃ at 5℃ / min to obtain the carbon material. Figure 4 As shown, its specific surface area is only 316.465m 2 g -1 , its average pore size is less than 1.5nm, and it only has microporous structure.

[0055] Comparative Example 2

[0056] The same method as in Example 1 is used, except that the polymer carbon source is polybenzimidazole.

[0057] Comparative Example 3

[0058] The same method as in Example 1 is used, except that the polymer carbon source is polystyrene.

[0059] Table 1 sample <![CDATA[BET(m 2 g -1 )]]> Average pore size (nm) Example 1 1769 4.9 Example 2 480 1.3 Example 3 1001 5.5 Example 4 501 1.4 Example 5 1054 2.8 Example 6 852 3.5 Example 7 1257 4.8 Example 8 1034 3.6 Comparative Example 1 412 1.2 Comparative Example 2 443 1.3 Comparative Example 3 459 1.2

[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a fuel cell catalyst carbon support, It is characterized in that include: Zinc citrate and polymer materials are used as raw materials and a fuel cell catalyst carbon carrier is obtained by step-wise high-temperature calcination; the polymer material is selected from one or more of polyacrylonitrile, polypyrrole, polyvinyl pyrrolidone, polyaniline and polydopamine.

2. The method for preparing a fuel cell catalyst carbon support according to claim 1, It is characterized in that The mass ratio of the zinc citrate to the polymer carbon source is 0.1:1 to 3:1; Preferably, the mass ratio of the zinc citrate to the polymer carbon source is 0.5:1 to 3:

1.

3. The method for preparing a fuel cell catalyst carbon support according to claim 1 or 2, It is characterized in that The step-by-step high-temperature calcination includes: heating to 600-700°C at a first heating rate, keeping the temperature for 1-4 hours, then heating to 800-1200°C at a second cooling rate, keeping the temperature for 1-4 hours, and then cooling to 300-350°C at a certain cooling rate.

4. The method for preparing a fuel cell catalyst carbon support according to claim 3, It is characterized in that The first heating rate is 2 to 20°C / min; and / or the second heating rate is 2 to 20°C / min; and / or the cooling rate is 2 to 10°C / min.

5. The method for preparing a fuel cell catalyst carbon support according to any one of claims 1 to 4, It is characterized in that The zinc citrate and the polymer material are ground for 10 to 30 minutes. Preferably, the high temperature calcination is carried out under an inert atmosphere; Preferably, nitrogen is introduced to provide an inert nitrogen atmosphere, and the gas flow rate is preferably 30 to 200 cc / min.

6. The method for preparing a fuel cell catalyst carbon support according to claim 1, It is characterized in that include: Grind zinc citrate and polydopamine for 10 to 30 minutes; The ground mixture is then heated in a stepwise manner under an inert atmosphere with an inert gas flow rate of 30 to 200 cc / min and a heating rate of 2 to 20°C / min. The temperature is first raised to 600 to 650°C and kept for 1 to 4 hours, then raised to 800 to 1200°C and kept for 1 to 4 hours; the temperature is then programmed to decrease at a rate of 2 to 10°C / min to 300 to 350°C, and then naturally decreased.

7. A fuel cell catalyst carbon support prepared by the method for preparing a fuel cell catalyst carbon support according to any one of claims 1 to 6.

8. Use of the fuel cell catalyst carbon support prepared by the preparation method according to any one of claims 1 to 6 or the fuel cell catalyst carbon support according to claim 7 in the preparation of fuel cell catalysts.

9. A fuel cell catalyst, It is characterized in that A fuel cell catalyst carbon support prepared by the preparation method according to any one of claims 1 to 6 or a fuel cell catalyst carbon support according to claim 7; Preferably, the platinum loading of the fuel cell catalyst is 20 wt% to 60 wt%.

10. The method for preparing the fuel cell catalyst according to claim 9, It is characterized in that include: The fuel cell catalyst carbon carrier is mixed with a chloroplatinic acid solution, water is added and ice bath ultrasound is performed, and then heating and magnetic stirring are performed, freeze drying and high temperature reduction are performed to obtain a fuel cell catalyst; preferably, the reduction temperature is 150-500° C. and the time is 1-3 hours.

Citation Information

Patent Citations

  • Array carbon nano-tube / graphene platinum-supported catalyst for fuel cell and preparation method of array carbon nano-tube / graphene platinum-supported catalyst

    CN104466204A

  • Preparation method of aniline through catalytic nitrobenzene hydrogenation

    CN105294447A

  • Fuel cell catalyst graphitized carbon carrier, preparation method thereof and fuel cell catalyst employing graphitized carbon carrier

    CN108649243A

  • Silver / carbon nanotube composite material and preparation method and application thereof

    CN109900758A

  • Catalyst of carbon fiber supported platinum-cobalt intermetallic compound as well as preparation method and application of catalyst

    CN116207282A

Cited By

  • Ionic liquid modification method of hydrogen fuel cell catalyst and slurry and membrane electrode thereof