Low-ash bamboo charcoal, bamboo-based hard charcoal negative electrode material and preparation method and application thereof
The inorganic components in bamboo materials, especially silicon, are removed through alkali soaking and pickling treatments, which solves the problem of difficulty in removing silicon in bamboo materials, improves the electrochemical properties of bamboo-based hard charcoal, and achieves efficient removal and electrochemistry of bamboo charcoal. Improved performance, simplicity and environmental protection.
Patent Information
- Application Number
- CN202410895140.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-29
AI Technical Summary
The inorganic components contained in bamboo and bamboo charcoal, especially silicon, are difficult to remove and affect the electrochemical performance of bamboo charcoal, bamboo-based activated carbon and bamboo-based hard carbon, and existing technology has not yet effectively solved this problem.
The alkali is loaded on the bamboo through alkali soaking. The alkali reacts with the inorganic matter in the bamboo at the carbonization temperature to generate water-soluble salts. After pickling, the silicon and other inorganic components in the bamboo are removed to prepare bamboo with excellent electrochemical properties. Based on hard carbon negative electrode material.
It effectively reduces the content of inorganic components in bamboo, especially the silicon content, from 0.3% to 0.5%, improves the electrochemical performance of bamboo-based hard carbon, simplifies the preparation process, is economical and environmentally friendly, and is suitable for large-scale applications .
Smart Images

Figure CN118851149A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of comprehensive utilization of biomass energy, in particular to the field of comprehensive utilization of bamboo materials, and specifically to a low-ash bamboo charcoal, a bamboo-based hard carbon negative electrode material, and a preparation method and application thereof. Background Art
[0002] Bamboo has a short growth cycle and is widely planted, so my country has extremely rich bamboo resources. At present, bamboo is used as a raw material to produce bamboo charcoal, bamboo activated carbon, bamboo-based hard carbon, etc. These porous carbon materials are widely used in the fields of environment and energy. However, bamboo is a silicon-rich body and contains many inorganic components mainly composed of silicon, which seriously affects the application performance of bamboo-based porous carbon materials. For example, bamboo is an excellent precursor for making hard carbon and can be used as a negative electrode material for batteries. For example, the invention patent with application number 202311052921.8 discloses bamboo-based hard carbon materials, their preparation, and their application in sodium ion batteries. The invention places the peeled bamboo tube in a modification liquid for liquid phase modification, and then roasts it in an oxygen-containing atmosphere for gas-solid modification. The modified bamboo tube is pre-carbonized to obtain a precursor, and then carbonized to obtain a bamboo-based hard carbon material. As a negative electrode active material, it exhibits relatively excellent electrochemical properties and uniformity. The invention patent with application number 202311682100.2 discloses a preparation method and application of a high-rate performance bamboo-based hard carbon negative electrode material. The method involves immersing bamboo powder in an inorganic salt solution, drying it, and calcining the resulting mixed powder in a protective atmosphere to obtain a hard carbon precursor. After cleaning, a bamboo-based hard carbon negative electrode active material is obtained, and a high-rate performance sodium ion battery negative electrode material can be obtained. However, the inorganic components remaining in the bamboo charcoal will cause problems such as high internal resistance and leakage, especially silicon will reduce conductivity, cover active sites, affect pore development, and hinder ion transport. Therefore, removing inorganic components from bamboo, especially removing silicon, is of great significance for the preparation of carbon materials such as hard carbon precursors.
[0003] The research on removing inorganic components from bamboo is in its infancy at home and abroad. The method of water leaching or acid washing bamboo can remove some inorganic components in bamboo, but the desiliconization effect has not yet been paid attention to. Chen et al. (Chen D, Zhuang X, Gan Z, et al. Co-pyrolysis of light bio-oil leached bamboo and heavy bio-oil: Effects of mass ratio, pyrolysis temperature, and residence time on the biochar [J]. Chemical Engineering Journal, 2022, 437: 135253) found that light bio-oil and heavy bio-oil fractions leached bamboo had a significant effect on removing K, Ca, Na, and Mg; Zhang Zhen et al. (Zhang Zhen, Yang Shengjie, Zhang Xiaoli, et al. Research on deashing process of bamboo-based activated carbon raw materials for supercapacitors [J]. Battery Industry, 2013, 18 (1 / 2): 55-57) first washed the bamboo with hot water and then soaked it in acid to obtain a better deashing effect. When the volume ratio of HNO3 to HCl was 2, the bamboo ash content could be removed to 0.53%, and the ash removal rate reached 87.3%. So far, there are few studies on the removal of silicon in bamboo. In fact, bamboo contains high levels of silicon, which often exists in the form of chemically stable silicon dioxide and is extremely difficult to remove. Summary of the invention
[0004] The technical problem solved by the present invention is that the inorganic components contained in bamboo and bamboo charcoal, especially silicon, have a great impact on the application of bamboo charcoal, bamboo-based activated carbon and bamboo-based hard carbon and are difficult to remove. It is urgent to develop a simple and efficient method for removing inorganic components from bamboo, especially silicon, which has a better removal effect. The electrochemical performance of bamboo-based hard carbon as a negative electrode material for batteries also needs to be improved.
[0005] The purpose of the present invention is to solve the problem of difficult removal of inorganic components, especially high silicon content, in the process of preparing carbon materials by carbonizing bamboo. The main advantage is that while effectively removing the silicon element in the bamboo, other inorganic components are removed to prepare a bamboo-based hard carbon negative electrode material with excellent electrochemical properties.
[0006] In order to solve the above technical problems, the present invention proposes a method for removing inorganic components mainly composed of silicon from bamboo. The method loads alkali on bamboo by alkali soaking. When the bamboo is carbonized, the alkali reacts with inorganic substances in the bamboo at the carbonization temperature to generate water-soluble salts, among which the alkali reacts with silicon to generate water-soluble silicates. After acid washing and water washing to neutrality, silicon and other inorganic components in bamboo can be effectively removed, thus overcoming the shortcomings and defects mentioned in the background technology.
[0007] Specifically, in view of the deficiencies of the prior art, the present invention provides the following technical solutions:
[0008] A low-ash bamboo charcoal, characterized in that the content of inorganic components in the bamboo charcoal is 0.50% to 1.50% of the bamboo charcoal, and the content of silicon in the bamboo charcoal is 3000 to 12500 mg / kg.
[0009] Preferably, in the above-mentioned low-ash bamboo charcoal, the content of inorganic components in the bamboo charcoal is 0.50% to 1.10%, more preferably 0.50% to 0.60%.
[0010] Preferably, the silicon content of the low-ash bamboo charcoal is 3000-8900 mg / kg, more preferably 3000-6500 mg / kg, and even more preferably 3000-3500 mg / kg.
[0011] Preferably, in the above-mentioned low-ash bamboo charcoal, the low-ash bamboo charcoal is prepared by a method comprising the following steps:
[0012] (1) Alkali treatment: immerse the bamboo in an aqueous solution of potassium hydroxide, filter, and dry;
[0013] (2) carbonization treatment: placing the bamboo material obtained in step (1) under an inert atmosphere at 600° C. to 750° C. to carbonize the bamboo material to obtain bamboo charcoal;
[0014] (3) Cleaning treatment: The bamboo charcoal is washed with acid and water in sequence, and then dried to obtain low-ash bamboo charcoal.
[0015] Preferably, in the above-mentioned low-ash bamboo charcoal, the carbonization temperature is 650-750°C, more preferably 630°C to 670°C.
[0016] Preferably, in the above-mentioned low-ash bamboo charcoal, the bamboo material is carbonized at 500-600°C for 1-2 hours, and the mass percentage of potassium element in the obtained bamboo charcoal is 23% to 27% of the total mass of inorganic component elements, the mass percentage of silicon element in the total mass of inorganic component elements is 15% to 20%, the content of potassium element in the bamboo charcoal is 12000 to 13000 mg / kg, and the content of silicon element in the bamboo charcoal is 12600 to 13000 mg / kg.
[0017] The present invention also provides a bamboo-based hard carbon negative electrode material, characterized in that it is prepared by a method comprising the following steps:
[0018] The low-ash bamboo charcoal is carbonized at 1200° C. to 1400° C. under an inert atmosphere to obtain a bamboo-based hard carbon negative electrode material.
[0019] Preferably, in the above-mentioned bamboo-based hard carbon negative electrode material, the carbonization temperature is 1200°C to 1300°C, more preferably 1280°C to 1320°C.
[0020] Preferably, in the above-mentioned bamboo-based hard carbon negative electrode material, the carbonization time of the bamboo-based hard carbon negative electrode active material is 2 to 3 hours, and the heating rate is 5 to 15° C. / min.
[0021] Preferably, the specific surface area of the bamboo-based hard carbon negative electrode material is 19 to 36 m 2 / g.
[0022] Preferably, the specific surface area of the bamboo-based hard carbon negative electrode material is 19 to 32 m 2 / g, more preferably 28 to 31 m 2 / g.
[0023] The present invention also provides a method for preparing low-ash bamboo charcoal, which is characterized by comprising the following steps:
[0024] (1) Alkali treatment: immerse the bamboo in an aqueous solution of potassium hydroxide, filter, and dry;
[0025] (2) carbonization treatment: placing the bamboo material obtained in step (1) under an inert atmosphere at 600° C. to 750° C. to carbonize the bamboo material to obtain bamboo charcoal;
[0026] (3) Cleaning treatment: The bamboo charcoal is washed with acid and water in sequence, and then dried to obtain low-ash bamboo charcoal.
[0027] Preferably, in the above-mentioned method for preparing low-ash bamboo charcoal, in the step (1), the concentration of the potassium hydroxide aqueous solution is 1 mol / L to 5 mol / L, preferably 2 mol / L to 4 mol / L; and the solid-to-liquid ratio of the bamboo material to the potassium hydroxide aqueous solution is 1 g:3 mL to 1 g:5 mL.
[0028] Preferably, in the method for preparing the low-ash bamboo charcoal, in the step (1), the immersion time is 2 h to 5 h, preferably 3 h to 4 h.
[0029] Preferably, in the above-mentioned method for preparing low-ash bamboo charcoal, in the method for preparing low-ash bamboo charcoal, in the step (2), the heating rate of the carbonization process is 5-15°C / min, and the carbonization time is 0.5-1.5h.
[0030] Preferably, in the above-mentioned method for preparing low-ash bamboo charcoal, the acid used in step (3) is hydrochloric acid with a concentration of 1 to 2 mol / L, and the solid-liquid ratio of bamboo charcoal to acid is 1 g:15 mL to 1 g:25 mL.
[0031] The present invention also provides a method for preparing a bamboo-based hard carbon negative electrode material, which is characterized by comprising the following steps:
[0032] The low-ash bamboo charcoal is carbonized at 1200° C. to 1400° C. under an inert atmosphere to obtain a bamboo-based hard carbon negative electrode material.
[0033] The present invention also provides a sodium ion battery negative electrode material, characterized in that it comprises the above-mentioned bamboo-based hard carbon negative electrode material.
[0034] The present invention also provides a sodium ion battery, characterized in that it comprises the above-mentioned sodium ion battery negative electrode material.
[0035] Preferably, the sodium ion battery has a reversible specific capacity of 250 to 385 mAh·g at a current density of 50 mA / g. -1 , preferably 280 to 385 mAh g -1 , more preferably 350 to 385 mAh·g -1 , more preferably 370 to 385 mAh·g -1 .
[0036] The present invention also provides the bamboo charcoal, the bamboo-based hard carbon negative electrode material, the sodium ion battery negative electrode material, or the use of the sodium ion battery in the field of energy storage materials.
[0037] The advantages of the present invention are: (1) the present invention can effectively remove most of the inorganic components in bamboo, mainly silicon, and the ash content can be reduced to about 0.50%, and the silicon content can be reduced to 0.3%; (2) after the bamboo charcoal is prepared into hard charcoal, it has excellent electrochemical properties as a negative electrode material for batteries, greatly improving the application value of the bamboo charcoal; (3) the preparation method of the bamboo charcoal and hard charcoal of the present invention is simple, and the amount of raw materials used is small. Under the premise of ensuring the deashing effect, the preparation process is economical and environmentally friendly, and has the potential for large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Schematic diagram of the content of various inorganic components in the bamboo charcoal BC obtained in Comparative Example 1.1.
[0039] Figure 2 Schematic diagram of the inorganic component content of the original bamboo material, bamboo charcoal obtained in Examples 1.1 to 1.8, and Comparative Example 1.1.
[0040] Figure 3 Schematic diagram of the inorganic component content of the bamboo charcoal obtained in Example 1.3 and Example 1.9 to Example 1.11.
[0041] Figure 4 Schematic diagram of the inorganic component content of the bamboo charcoal obtained in Examples 1.1 to 1.11 and Comparative Example 1.1.
[0042] Figure 5 This is the cyclic voltammogram of the bamboo-based hard carbon obtained in Example 2.1.
[0043] Figure 6 This is the rate performance diagram of the bamboo-based hard charcoal obtained in Example 2.1.
[0044] Figure 7 This is the AC impedance diagram of the bamboo-based hard carbon obtained in Example 2.1. DETAILED DESCRIPTION
[0045] As a biomass resource that has been vigorously developed in recent years, bamboo charcoal obtained by carbonization and bamboo activated carbon obtained after further activation have been widely used in the fields of adsorption separation, energy storage, etc. In addition, bamboo charcoal also has the natural advantage of preparing hard carbon precursors. However, the inorganic components contained in bamboo and bamboo charcoal, especially silicon, have a great impact on the application of bamboo charcoal and bamboo activated carbon and are difficult to remove. The present invention provides a method for deep removal of inorganic components in the process of preparing bamboo charcoal, bamboo-based activated carbon and bamboo-based hard charcoal using bamboo as raw material. It relates to the field of bamboo charcoal utilization, and specifically to a low-ash bamboo charcoal, bamboo-based hard charcoal negative electrode material, and its preparation method and application.
[0046] In a preferred embodiment, the method for removing inorganic components from bamboo material of the present invention comprises the following steps:
[0047] The bamboo was crushed and soaked in a 3 mol / L KOH solution for 4 hours, with a solid-liquid ratio of 1g:3ml. After soaking, the bamboo was filtered out and placed in a vacuum blast drying oven at 105°C for 12 hours. The dried bamboo was carbonized for 1 hour in a nitrogen atmosphere, with a carbonization temperature of 650°C and a heating rate of 10°C / min. The carbonized bamboo was ground through a 1mm sieve, and washed with 1 mol / L hydrochloric acid at a solid-liquid ratio of 1g:20ml for 1 hour. After washing, the carbon powder was washed with deionized water until it was neutral. The carbon powder was filtered out and dried to obtain bamboo charcoal, and a low-ash bamboo charcoal with an ash content of 0.55% was obtained, in which the silicon content was reduced from 1.26% (ICP measured the Si content in the original bamboo charcoal) to 0.3%. The desiliconization rate reached 76.19%.
[0048] In the present invention, the alkali solution used is a KOH solution, and K can react with Si to form potassium silicate, converting silicon in the form of silicon dioxide into soluble silicate. After research, the inventors found that if the alkali solution is a NaOH solution, the sodium content in the bamboo charcoal will increase. Compared with Na, the K in KOH has a higher reaction activity and is easier to react with SiO2. In addition, K is more conducive to the development of the pore structure of the carbon material during the carbonization process, and the specific surface area of the carbon material is increased by pore formation, so that the inorganic components in the carbon matrix are more fully exposed, which is more conducive to the removal of inorganic components. In addition, most of K still exists in a soluble state after carbonization and is easy to remove, while Na will react and combine with the carbon matrix during the carbonization process, which increases the difficulty of removing inorganic components and affects the electrochemical properties of the hard carbon negative electrode material.
[0049] In the present invention, the inert atmosphere refers to nitrogen or argon.
[0050] The low-ash bamboo charcoal and bamboo-based hard carbon negative electrode materials of the present invention and their preparation methods and applications are further described below through specific examples.
[0051] In the following examples, the information of the reagents and instruments used is shown in the following table, and other reagents are purchased from Sinopharm Group. The bamboo material used in the examples of the present invention is 3-year-old moso bamboo, which is selected from bamboo processing waste and has an ash content of 1.0%-1.5%.
[0052] Table 1 Equipment and reagent information
[0053]
[0054] Example 1 Preparation of bamboo charcoal
[0055] Example 1.1
[0056] The bamboo was crushed into 6 meshes, immersed in 1mol / L KOH solution for 4 hours, with a solid-liquid ratio of 1g:3ml, filtered out, placed in a vacuum blast drying oven, and dried at 105℃ for 12 hours. The dried bamboo was placed in a tubular furnace and carbonized under a nitrogen atmosphere. The heating rate of the tubular furnace was 10℃ / min, the carbonization temperature was 600℃, and the carbonization time was 1 hour to obtain bamboo charcoal. The bamboo charcoal was ground through a 1mm sieve, 1mol / L hydrochloric acid solution was added, with a solid-liquid ratio of 1g:20ml, stirred for 1 hour, washed with deionized water until neutral, filtered and dried to obtain low-ash bamboo charcoal, marked as BC-1.
[0057] Example 1.2
[0058] Similar to Example 1.1, except that the concentration of KOH solution was adjusted to 2 mol / L, and the obtained low-ash bamboo charcoal was marked as BC-2.
[0059] Example 1.3
[0060] Similar to Example 1.1, except that the concentration of KOH solution was adjusted to 3 mol / L, and the obtained low-ash bamboo charcoal was marked as BC-3.
[0061] Example 1.4
[0062] Similar to Example 1.1, except that the concentration of KOH solution was adjusted to 4 mol / L, and the obtained low-ash bamboo charcoal was marked as BC-4.
[0063] Example 1.5
[0064] The bamboo was crushed into 6 meshes, immersed in 5mol / L KOH solution for 4 hours, with a solid-liquid ratio of 1g:3ml, filtered out, placed in a vacuum blast drying oven, and dried at 105℃ for 12 hours. The dried bamboo was placed in a tubular furnace and carbonized under a nitrogen atmosphere. The heating rate of the tubular furnace was 5℃ / min, the carbonization temperature was 600℃, and the carbonization time was 1.5 hours to obtain bamboo charcoal. The bamboo charcoal was ground through a 1mm sieve, and a 2mol / L hydrochloric acid solution was added, with a solid-liquid ratio of 1g:25ml, stirred for 1 hour, washed with deionized water until neutral, filtered and dried to obtain low-ash bamboo charcoal, marked as BC-5.
[0065] Example 1.6
[0066] The bamboo was crushed into 6 meshes, immersed in 3mol / L KOH solution for 2 hours, with a solid-liquid ratio of 1g:3ml, filtered out, placed in a vacuum blast drying oven, and dried at 105℃ for 12 hours. The dried bamboo was placed in a tubular furnace and carbonized under a nitrogen atmosphere. The heating rate of the tubular furnace was 10℃ / min, the carbonization temperature was 600℃, and the carbonization time was 1 hour to obtain bamboo charcoal. The bamboo charcoal was ground through a 1mm sieve, 1mol / L hydrochloric acid solution was added, with a solid-liquid ratio of 1g:20ml, stirred for 1 hour, washed with deionized water until neutral, filtered and dried to obtain low-ash bamboo charcoal, marked as BC-2h.
[0067] Example 1.7
[0068] The bamboo was crushed into 6 meshes, immersed in 3 mol / L KOH solution for 3 hours, with a solid-liquid ratio of 1g:3ml, filtered out, placed in a vacuum blast drying oven, and dried at 105℃ for 12 hours. The dried bamboo was placed in a tubular furnace and carbonized under a nitrogen atmosphere. The heating rate of the tubular furnace was 10℃ / min, the carbonization temperature was 600℃, and the carbonization time was 1 hour to obtain bamboo charcoal. The bamboo charcoal was ground through a 1mm sieve, 1 mol / L hydrochloric acid solution was added, with a solid-liquid ratio of 1g:20ml, stirred for 1 hour, washed with deionized water until neutral, filtered and dried to obtain low-ash bamboo charcoal, marked as BC-3h.
[0069] Example 1.8
[0070] The bamboo was crushed into 6 meshes, immersed in 3 mol / L KOH solution for 5 hours, with a solid-liquid ratio of 1g:5ml, filtered out, placed in a vacuum blast drying oven, and dried at 105°C for 12 hours. The dried bamboo was placed in a tubular furnace and carbonized under a nitrogen atmosphere. The heating rate of the tubular furnace was 15°C / min, the carbonization temperature was 600°C, and the carbonization time was 0.5 hours to obtain bamboo charcoal. The bamboo charcoal was ground through a 1mm sieve, 1 mol / L hydrochloric acid solution was added, with a solid-liquid ratio of 1g:15ml, stirred for 1 hour, washed with deionized water until neutral, filtered and dried to obtain low-ash bamboo charcoal, and the obtained bamboo charcoal was marked as BC-5h.
[0071] Example 1.9
[0072] Similar to Example 1.3, the difference is that the carbonization temperature is adjusted to 650°C, and the obtained low-ash bamboo charcoal is marked as BC-650°C.
[0073] Example 1.10
[0074] Similar to Example 1.3, the difference is that the carbonization temperature is adjusted to 700°C, and the obtained low-ash bamboo charcoal is marked as BC-700°C.
[0075] Example 1.11
[0076] Similar to Example 1.3, the difference is that the carbonization temperature is adjusted to 750°C, and the obtained low-ash bamboo charcoal is marked as BC-750°C.
[0077] Comparative Example 1.1
[0078] The bamboo was crushed into 6 meshes, placed in a tubular furnace, and carbonized under a nitrogen atmosphere. The heating rate of the tubular furnace was 10°C / min, the carbonization temperature was 600°C, and the carbonization time was 1 hour to obtain bamboo charcoal, which was marked as BC. The bamboo charcoal BC was ground to 1mm, 1mol / L hydrochloric acid was added, and the solid-liquid ratio was 1g:20ml, stirred for 1 hour, washed with deionized water until neutral, and dried to obtain bamboo charcoal BC-0.
[0079] The bamboo charcoal obtained in the examples and comparative examples was characterized by: (1) elemental analysis by XRF; (2) elemental analysis by ICP; (3) ash content (or inorganic component content) was measured according to the ash content test method in the national standard "Bamboo Charcoal" GB / T26913-2011; (4) nitrogen adsorption and desorption isotherms of bamboo charcoal were measured by pore size and specific surface area analyzer, and the specific surface area of bamboo charcoal was calculated by BET equation.
[0080] The XRF analysis results of various inorganic elements in the bamboo charcoal BC obtained by carbonization of raw bamboo are as follows: Figure 1 As shown, the ordinate is the mass percentage of each element in the total amount of inorganic components. Figure 1It can be seen that the content of alkali metals / alkaline earth metals in the inorganic components of bamboo charcoal accounts for a large proportion, the content of K is the highest, and the content of Si is also relatively high, accounting for 16.10%.
[0081] According to GB / T26913-2011, the inorganic component content of the original bamboo (Bamboo) was detected. The inorganic component content of the bamboo charcoal obtained in Examples 1.1 to 1.8 and Comparative Example 1.1 was as follows: Figure 2 As shown, the ordinate is the percentage of the total amount of inorganic elements in the mass of bamboo charcoal. Comparing BC and the original bamboo material, it can be seen that the inorganic content of the bamboo material is significantly increased after carbonization. Comparing BC and BC-0, it can be seen that after the bamboo charcoal is pickled, the inorganic component content is significantly reduced, which can be reduced from 3.61% to 2.73%; in Examples 1.1 to 1.8, the inorganic component content of the bamboo charcoal after alkali leaching and carbonization and then pickling can reach less than 1.5%, and in Example 3, when the KOH concentration is 3 mol / L and the immersion time is 4h, the ash content of the obtained bamboo charcoal can be as low as 0.91%.
[0082] According to GB / T26913-2011, the inorganic component content of the bamboo charcoal obtained in Example 1.3, Example 1.9 to Example 1.11 is as follows: Figure 3 As shown in the figure, it can be seen that in Example 1.9, after the bamboo charcoal was impregnated with 3 mol / L KOH solution for 4 hours and then carbonized at 650°C, the inorganic component content of the obtained bamboo charcoal was extremely low, reaching 0.55%. Compared with BC, the deashing rate was 84.76%.
[0083] ICP was used to detect the inorganic component content of the bamboo charcoal obtained in Examples 1.1 to 1.11. Figure 4 As shown, the content of inorganic components represents the mass of each element in each kilogram of bamboo charcoal. It can be seen from the figure that the silicon content of BC is 12625 mg / kg, the silicon content of BC-0 is 11960.7 mg / kg, the silicon content of bamboo charcoal in Examples 1.1 to 1.5 is 8315.6 mg / kg, 7743.5 mg / kg, 6601.1 mg / kg, 7070.1 mg / kg, 8834.0 mg / kg, the silicon content of bamboo charcoal in Examples 1.6 to 1.8 is 10360.0 mg / kg, 10053.9 mg / kg, 12137.8 mg / kg, and the silicon content of bamboo charcoal in Examples 1.9 to 1.11 is 3011.4 mg / kg, 3387.5 mg / kg, 3390.6 mg / kg. For elements other than silicon, the removal effect is also very obvious. Taking Example 1.3, Example 1.9, Example 1.10, and Example 1.11 as examples, the contents of other elements are shown in Table 2.
[0084] Table 2 Element content of bamboo charcoal obtained in the embodiment
[0085]
[0086] Comparing BC and BC-0, it can be seen that pickled bamboo charcoal can have obvious removal effects on K, Ca, Na, Mg, etc., and the changes in K and Ca are particularly obvious, indicating that K and Ca mostly exist in water-soluble and acid-soluble states, while Mg and Na mostly exist in combined states, which are relatively difficult to remove K and Ca; Si occupies a major part in the inorganic components of bamboo charcoal, and the Si element content accounts for 1.26% of the mass of bamboo charcoal. And the content of Si in the bamboo charcoal after pickling changes very little, indicating that it is difficult to remove the main element Si in the inorganic components of bamboo charcoal by pickling alone. Comparing the embodiments and comparative examples, it can be seen that the content of silicon in the inorganic components of bamboo charcoal treated by KOH impregnation is significantly reduced, and the KOH loaded on the bamboo will react with the silicon in the bamboo to form silicate during the carbonization process, so that it can be effectively removed in the subsequent pickling. In Example 1.9, the proportions of various elements in the bamboo charcoal BC-650℃ treated with 3mol / L KOH solution for 4h and carbonization temperature of 650℃ were relatively low, and the silicon content decreased from 1.26% to 0.3%. The removal rate can reach 76.19%, which is comparable to Figure 2 , Figure 3 The results are consistent.
[0087] Example 2 Preparation and Application of Hard Carbon
[0088] Example 2.1
[0089] The deashed bamboo charcoal obtained in Example 1.9 was placed in a tubular furnace, heated at a rate of 5°C / min under a nitrogen atmosphere, and carbonized at a carbonization temperature of 1300°C for 2 h to obtain hard charcoal.
[0090] The specific surface area of hard carbon was 31.06 m 2 ·g -1 .
[0091] The cyclic voltammetry curve of the obtained sodium ion battery was detected. The detection process was as follows: the bamboo charcoal material, the conductive agent (acetylene black) and the binder (polytetrafluoroethylene PVDF) were mixed in a mass ratio of 8:1:1, and NIP (Nafion polymer) was used as a dispersant to prepare a paste slurry. The slurry was coated on a copper foil and dried at 80°C in a forced air drying oven for 12 hours. The dried electrode sheet was punched into a circular working electrode sheet with a diameter of 14 mm for standby use. The battery was assembled in an argon glove box with moisture and oxygen less than 0.01 mg / L, respectively. A CR2032 battery shell was used, and the electrolyte was a sodium ion battery electrolyte (1 mol / L NaPF6 in ethylene carbonate + dimethyl carbonate (volume ratio of 1:1)). The metal sodium sheet was used as both the counter electrode and the reference electrode, and a glass fiber diaphragm was used as the diaphragm. The battery was assembled in the order of the positive electrode shell, the working electrode, the diaphragm, the metal sodium sheet, the gasket, the shrapnel and the negative electrode shell from bottom to top, and the electrochemical performance was detected by the blue electric system. The results are as follows Figure 5 As shown in the figure, the high overlap of the three cycle curves indicates that the solid electrolyte interface (SEI) consumes less electrolyte and the irreversible sodium insertion behavior on the hard carbon surface is less, and the hard carbon has good reversibility as an electrode material. The high voltage slope area corresponds to the storage of sodium ions at the surface sites, while the low voltage slope area corresponds to the insertion of sodium ions between the carbon layers. The highly overlapping CV curves confirm that Na + The reversible insertion and extraction of ions in the hard carbon structure indicate that the prepared hard carbon anode material has excellent stability and reversibility.
[0092] The obtained hard carbon was subjected to constant current charge and discharge tests at 25°C with the current density increased from 50 mA / g to 2 A / g, and the rate performance diagram was obtained, as shown in FIG. Figure 6 When the current density is 50mA / g, 100mA / g, 200mA / g, 500mA / g, 1A / g, and 2A / g, the reversible specific capacity of the battery is 384.4mAh·g -1 、371.1mAh·g -1 、358.4mAh·g -1 、336mAh·g -1 、287.9mAh·g -1 , 202.9mAh·g -1 When the current density is restored to 50mA / g, it can still be restored to 365mAh·g -1 The specific capacity shows excellent rate performance.
[0093] The AC impedance diagram of hard carbon material is as follows Figure 7 As shown, the best impedance performance graph should be a semicircle with a small diameter, which means that the resistance of the electrode material is small and has better electrochemical performance. Figure 7The characterization shows an arc shape, which is due to the uneven surface of the electrode and the formation of a solid electrolyte interface film, which is a characteristic of porous carbon materials. In addition, it can be seen that the smaller arc shape indicates that the hard carbon material has a smaller charge transfer resistance and can provide excellent electrochemical performance.
[0094] On the basis of Example 2.1, the carbonization temperature of Example 1.9 was adjusted to 630°C to obtain bamboo charcoal BC-630°C, and then carbonized at 1280°C for 3h under nitrogen atmosphere at a heating rate of 10°C / min to obtain hard carbon negative electrode active material. It was assembled into a sodium ion battery according to the steps of Example 2.1, and the electrochemical performance was measured. At a current density of 50mA / g, the reversible specific capacity can reach 382.3mAh·g -1 .
[0095] On the basis of Example 2.1, the carbonization temperature of Example 1.9 was adjusted to 670°C to obtain bamboo charcoal BC-670°C, and then carbonized at 1320°C for 2h under nitrogen atmosphere at a heating rate of 10°C / min to obtain a hard carbon negative electrode active material. It was assembled into a sodium ion battery according to the steps of Example 2.1, and the electrochemical performance was measured. At a current density of 50mA / g, the reversible specific capacity can reach 381.7mAh·g -1 .
[0096] Example 2.2
[0097] The deashed bamboo charcoal obtained in Example 1.9 was placed in a tubular furnace, heated at a rate of 5°C / min under a nitrogen atmosphere, and carbonized at 1200°C for 2h to obtain hard charcoal.
[0098] The specific surface area of hard carbon was 31.94 m 2 ·g -1 .
[0099] The obtained hard carbon was assembled into a sodium ion battery according to the method of Example 2.1, and its electrochemical performance was tested. The results showed that when the current density was 50mA / g, 100mA / g, 200mA / g, 500mA / g, 1A / g, and 2A / g, the reversible specific capacity of the battery was 271.6mAh·g -1 、256.6mAh·g -1 、247.1mAh·g -1 、231.3mAh·g -1 、211.3mAh·g -1 、170mAh·g -1 When the current density is restored to 50 mA / g, the specific capacity can be restored to 251.8 mAh g -1 .
[0100] Example 2.3
[0101] The deashed bamboo charcoal obtained in Example 1.9 was placed in a tubular furnace, heated at a rate of 5°C / min under a nitrogen atmosphere, and carbonized at 1400°C for 2h to obtain hard charcoal.
[0102] The specific surface area of the hard carbon was 19.22 m 2 ·g -1 .
[0103] The obtained hard carbon was assembled into a sodium ion battery according to the method of Example 2.1, and its electrochemical performance was tested. The results showed that when the current density was 50mA / g, 100mA / g, 200mA / g, 500mA / g, 1A / g, and 2A / g, the reversible specific capacity of the battery was 243mAh·g -1 、224.8mAh·g -1 、198mAh·g -1 、140.2mAh·g -1 、69.2mAh·g -1 , 25.2mAh·g -1 When the current density is restored to 50 mA / g, the specific capacity can be restored to 215.3 mAh g -1 .
[0104] Example 2.4
[0105] The bamboo charcoals obtained in Examples 1.1 to 1.8, 1.10 and 1.11 were prepared into hard charcoal according to the method described in Example 2.1.
[0106] The specific surface area was tested by pore size and specific surface area analyzer. The results showed that the specific surface areas of the hard charcoal prepared by bamboo charcoal in Examples 1.1 to 1.8, 1.10 and 1.11 were 20.41 m 2 ·g -1 、23.15m 2 ·g -1 、28.72m 2 ·g -1 、33.05m 2 ·g -1 、35.42m 2 ·g -1 、22.91m 2 ·g -1 、24.27m 2 ·g -1 、26.72m 2 ·g -1 、30.28m 2 ·g -1、29.51m 2 ·g -1 .
[0107] The electrochemical performance was tested. The results showed that when the current density was 50 mA / g, the reversible specific capacity of the hard carbon prepared from bamboo charcoal in Examples 1.1 to 1.8, 1.10 and 1.11 was 260 mAh·g -1 、263.4mAh·g -1 、284.7mAh·g -1 、280.5mAh·g -1 、273.7mAh·g -1 、280.4mAh·g -1 、256.2mAh·g -1 、251.7mAh·g -1 、376.5mAh·g -1 、375.9mAh·g -1 .
[0108] Comparative Example 2.1
[0109] The bamboo charcoal BC obtained in Comparative Example 1.1 was prepared into hard charcoal according to the method of Example 2.1.
[0110] The specific surface area of the hard carbon was 9.49 m 2 ·g -1 .
[0111] The hard carbon was used as the negative electrode material and assembled into a sodium ion battery according to the method of Example 2.1. The electrochemical performance was tested. The results showed that when the current density was 50 mA / g, 100 mA / g, 200 mA / g, 500 mA / g, 1 A / g, and 2 A / g, the reversible specific capacity of the battery was 258.4 mAh·g -1 、236.4mAh·g -1 、213.4mAh·g -1 、169mAh·g -1 、119.4mAh·g -1 、62.6mAh·g -1 When the current density is restored to 50 mA / g, the specific capacity can be restored to 228.8 mAh g -1 .
[0112] In summary, the bamboo charcoal and hard charcoal prepared by the present invention can be used as negative electrode active materials of sodium ion batteries to improve the electrochemical performance of sodium ion batteries. The preparation method of the present invention is simple and environmentally friendly and has the potential for large-scale application.
Claims
1. A low-ash bamboo charcoal, characterized in that: The content of inorganic components in the bamboo charcoal is 0.50% to 1.50% of the total content of the bamboo charcoal, and the content of silicon in the bamboo charcoal is 3000 to 12500 mg / kg of the total content of the bamboo charcoal.
2. The low-ash bamboo charcoal according to claim 1, wherein: The low-ash bamboo charcoal is prepared by a method comprising the following steps: (1) Alkali treatment: immerse the bamboo in an aqueous solution of potassium hydroxide, filter, and dry; (2) carbonization treatment: placing the bamboo material obtained in step (1) under an inert atmosphere at 600° C. to 750° C. to carbonize the bamboo material to obtain bamboo charcoal; (3) Cleaning treatment: The bamboo charcoal is washed with acid and water in sequence, and then dried to obtain low-ash bamboo charcoal.
3. A bamboo-based hard carbon negative electrode material, characterized in that: Prepared by a method comprising the following steps: The low-ash bamboo charcoal according to claim 1 or 2 is carbonized at 1200° C. to 1400° C. under an inert atmosphere to obtain a bamboo-based hard carbon negative electrode material.
4. The bamboo-based hard carbon negative electrode material according to claim 3, wherein: The specific surface area of the bamboo-based hard carbon negative electrode material is 19 to 36 m 2 / g.
5. A method for preparing low-ash bamboo charcoal, characterized in that: The steps include: (1) Alkali treatment: immerse the bamboo in an aqueous solution of potassium hydroxide, filter, and dry; (2) carbonization treatment: placing the bamboo material obtained in step (1) under an inert atmosphere at 600° C. to 750° C. to carbonize the bamboo material to obtain bamboo charcoal; (3) Cleaning treatment: The bamboo charcoal is washed with acid and water in sequence, and then dried to obtain low-ash bamboo charcoal.
6. The preparation method according to claim 5, wherein: In the step (1), the concentration of the potassium hydroxide aqueous solution is 1 mol / L to 5 mol / L; and the solid-liquid ratio of the bamboo material to the potassium hydroxide aqueous solution is 1 g:3 mL to 1 g:5 mL.
7. The preparation method according to claim 5 or 6, wherein: In the step (1), the immersion time is 2 hours to 5 hours.
8. A sodium ion battery negative electrode material, characterized in that: Contains the bamboo-based hard carbon negative electrode material as described in claim 3.
9. A sodium ion battery, characterized in that: Contains the sodium ion battery negative electrode material according to claim 8.
10. Use of the bamboo charcoal according to claim 1 or 2, the bamboo-based hard carbon negative electrode material according to claim 3 or 4, the sodium ion battery negative electrode material according to claim 8, or the sodium ion battery according to claim 9 in the field of energy storage materials.
Citation Information
Cited By
High-first-effect high-capacity bamboo-based hard carbon material and preparation method thereof
CN120149403A
Bamboo-based derived nitrogen-doped hard carbon negative electrode material and preparation method and application thereof
CN121823535A