Green and environment-friendly nano carbon dot corrosion inhibitor as well as preparation method and application thereof

The green and environmentally friendly nano nitrogen-doped carbon dot corrosion inhibitor synthesized by hydrothermal method uses the chemical stability of isoniazid and pyridine nitrogen functional group to solve the problems of corrosion of metal pipelines in hydrochloric acid solution and environmental pollution of organic corrosion inhibitors. , achieving high-efficiency, low-cost corrosion inhibition performance and providing effective protection for low carbon steel.

CN118851159APending Publication Date: 2024-10-29CHANGZHOU UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410899401.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the existing technology, there is a problem of corrosion of metal pipelines in a hydrochloric acid solution environment, and most organic corrosion inhibitors have a negative impact on the environment, are costly, and have poor corrosion inhibition performance.

Method used

A green and environmentally friendly nano nitrogen-doped carbon dot corrosion inhibitor prepared from citric acid and isoniazid is synthesized by hydrothermal method. The good chemical stability of isoniazid and pyridine nitrogen are used to improve the corrosion inhibition performance, and a one-step synthesis method is used. Reduce costs and environmental pollution.

Benefits of technology

It achieves significantly improved corrosion inhibition performance on the surface of low carbon steel, reduces synthesis costs and environmental pollution, and shows good anti-corrosion effects in sodium chloride solution, providing a safer and more environmentally friendly anti-corrosion solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851159A_ABST
    Figure CN118851159A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of nano corrosion inhibitors, and discloses a green and environment-friendly nano carbon dot corrosion inhibitor as well as a preparation method and application thereof. The preparation method comprises the following steps: respectively dissolving citric acid and isoniazide in deionized water, and reacting at 160 DEG C for 6 hours to obtain the green nano corrosion inhibitor as shown in formula (1). The corrosion inhibitor structurally contains a large number of nitrogen elements and hydroxyl groups and has good corrosion inhibition performance, the effect of the corrosion inhibitor is improved by doping the nitrogen elements, and the green and environment-friendly nano carbon dot corrosion inhibitor is adsorbed on the surface of metal in a physical adsorption and chemical adsorption combined adsorption mode, so that the corrosion inhibition effect is improved. Static corrosion inhibition effect evaluation proves that the corrosion inhibition performance of the corrosion inhibitor can reach up to 91.9%, and the corrosion inhibitor has good static corrosion inhibition performance. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano corrosion inhibitors, in particular to a green and environmentally friendly nano carbon dot corrosion inhibitor and a preparation method thereof. Technical Background

[0002] The corrosion of metal pipes in hydrochloric acid solution environment has always been a problem that plagues the development of the oil and gas industry. When the acid solution comes into contact with the metal surface, the metal will also be converted into water-soluble chlorides, so the surface begins to corrode. The acid solution will actively dissolve the surface of the substrate, and the structural integrity of the metal surface will be damaged. As a result, the carbon steel will corrode, causing the performance of the carbon steel to deteriorate and causing safety accidents.

[0003] As the main anti-corrosion technology, corrosion inhibitors have been widely used in actual production. Corrosion inhibitors made of nano-carbon dot materials are widely used due to their excellent properties such as good water solubility, easy modification, low cost, stability and environmental friendliness. Nano-carbon dot corrosion inhibitor is a corrosion inhibitor suitable for corrosion in neutral salt solutions. Isoniazid has pyridine nitrogen and amino groups in its structure, which is suitable as a nitrogen source for corrosion inhibitors. Nitrogen elements are doped into carbon dots through hydrothermal synthesis reaction to form nitrogen-doped nano-carbon dot corrosion inhibitors.

[0004] Patent CN202211226363.8 discloses a nitrogen-doped carbon quantum dot corrosion inhibitor, which uses ammonium citrate as a carbon source and thiourea as a doping nitrogen source, the mass ratio of ammonium citrate to thiourea is 3.5-4.5:1, and ethanol is used as a solvent. It is synthesized by hydrothermal method. The synthesis temperature is 180-200°C, the heating time is 15-18h, and the nitrogen-doped carbon quantum dot corrosion inhibitor is obtained after centrifugation and dialysis treatment and purification. Patent CN202311247818.9 discloses a green corrosion inhibitor, which uses citric acid as a carbon source, urea as a doping nitrogen source, and deionized water as a solvent. It is synthesized by hydrothermal method. After the obtained solution is centrifuged, filtered and dried, the desired nitrogen-doped carbon quantum dot corrosion inhibitor is obtained. Patent CN116376642A discloses an environmentally friendly nano-insulator cleaning agent, which comprises the following steps: adding 1-3g of citric acid and 0.5-1g of ethylenediamine into 30-50ml of water and completely dissolving them; placing the obtained solution into a microwave device and subjecting it to microwave treatment; freeze-drying the nitrogen-doped citric acid carbon quantum dots after microwave treatment to obtain a solid powder; as a green insulator cleaning agent, it has little harm to human body and environment, extremely low conductivity, high operational safety, and is non-corrosive to rubber, ceramics and metals.

[0005] Compared with the existing nitrogen-doped nano-carbon dot corrosion inhibitor, the nitrogen source selected by the present invention is isoniazid. Compared with ethylenediamine, isoniazid is relatively stable at room temperature, has good chemical stability, and is easy to obtain. At the same time, compared with ethylenediamine, it has a rich nitrogen source. In terms of structure, isoniazid not only has amino groups, but also has pyridine nitrogen, and pyridine nitrogen has a good corrosion inhibition effect. The corrosion inhibition performance of the synthetic corrosion inhibitor can be improved. Compared with the synthesis of nitrogen-doped nano-carbon dot corrosion inhibitors using melamine as a nitrogen source by a two-step hot solvent method, the present invention is significantly more efficient by a one-step hydrothermal synthesis method, and most of the synthesis methods have higher temperatures than the present invention, and the synthesis cost is high. Melamine has the disadvantages of toxicity, environmental pollution, and possible health problems. When using it, its risks should be carefully assessed, and effective measures should be taken to reduce its impact on human health and the environment. Isoniazid is non-toxic to the human body at a certain amount, and its waste liquid is also easy to handle and environmentally friendly. Laboratory operation is also more convenient and the synthesis efficiency is high. Summary of the invention

[0006] The present invention mainly overcomes the negative impact of most current organic corrosion inhibitor products or raw materials on the environment, and the high cost of organic corrosion inhibitors and poor corrosion inhibition performance in some cases. And the performance of nano corrosion inhibitors is improved by doping nitrogen elements. Nano carbon dot corrosion inhibitors are adsorbed on the surface of carbon steel by combining physical adsorption and chemical adsorption of different functional groups to protect carbon steel from corrosion. Moreover, green nano carbon corrosion inhibitors are lower in cost and more environmentally friendly than organic corrosion inhibitors.

[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0008] A green and environmentally friendly nano nitrogen-doped carbon dot corrosion inhibitor, the structural formula of which is shown in formula (1).

[0009]

[0010] A green and environmentally friendly nano nitrogen-doped carbon dot corrosion inhibitor is synthesized by a hydrothermal method using citric acid and isoniazid as raw materials.

[0011] The reaction process is shown in formula (2):

[0012]

[0013] A method for preparing a green and environmentally friendly nano nitrogen-doped carbon dot corrosion inhibitor comprises the following steps: weighing citric acid and isoniazid, adding deionized water to dissolve and mix to obtain a mixed solution, transferring the obtained mixed solution to a hydrothermal reactor, placing the reactor in a forced air drying oven to heat and perform a hydrothermal reaction, and cooling the obtained product to room temperature after the reaction; performing a dialysis treatment in deionized water, drying the obtained nitrogen-doped carbon nanoparticle solution, and obtaining nano nitrogen-doped carbon dot corrosion inhibitor solid particles.

[0014] Furthermore, the molar ratio of citric acid to isoniazid is 2:1 to 3. Preferably, the molar ratio of citric acid to isoniazid is 2:3.

[0015] Furthermore, the hydrothermal reaction conditions are: 140-180° C. for 4-8 hours. Preferably, the hydrothermal reaction conditions are 160° C. for 6 hours.

[0016] Furthermore, the obtained product was dialyzed in deionized water for 48 hours; during the dialysis, a dialysis bag with a molecular weight of 1000 MD was selected for dialysis and was changed every four hours.

[0017] Furthermore, the carbon nanoparticle solution was dried at 60° C. for 24 h.

[0018] Furthermore, the prepared nano corrosion inhibitor is in the form of solid powder.

[0019] Preparation of green and environmentally friendly nano-carbon dot corrosion inhibitors for application in metal corrosion protection.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The raw materials of the invention are easy to obtain, the synthesis method is simple, the conditions are mild, and the synthesis cost is low compared to organic corrosion inhibitors. Compared with traditional corrosion inhibitors, the nano carbon dot corrosion inhibitor is green and pollution-free, and has a better corrosion inhibition effect on low carbon steel in sodium chloride solution. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Infrared spectrum test of nano nitrogen doped carbon dots corrosion inhibitor.

[0023] Figure 2 This is the corrosion inhibition efficiency diagram of nano nitrogen doped carbon dots corrosion inhibitor. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] A method for preparing a green nano corrosion inhibitor, specifically comprising the following steps:

[0027] S1: Weigh citric acid and isoniazid (molar ratio 2:3) according to a weight ratio of 0.38:0.411;

[0028] S2: Put the medicine weighed in S1 into a beaker and add 20 ml of deionized water to dissolve and mix;

[0029] S3: The mixed solution obtained in S2 was transferred to a 50 ml polytetrafluoroethylene-lined hydrothermal reactor, the reactor was placed in a forced air drying oven and heated at 160°C for 6 hours, and then the obtained product was cooled to room temperature; S4: The product obtained in S3 was dialyzed in deionized water for 48 hours (molecular weight 1000MD).

[0030] Deionized water was changed every four hours;

[0031] S5: The carbon nano corrosion inhibitor particle solution obtained in S4 is transferred to a vacuum drying oven and dried at 60° C. for 24 hours to finally obtain the product.

[0032] The obtained product was subjected to Fourier infrared spectroscopy test to obtain Figure (2). Figure 2 The nitrogen element can be obtained from the corrosion inhibitor and has been successfully doped into the corrosion inhibitor. By doping with nitrogen, the corrosion inhibition performance of the corrosion inhibitor is improved by forming a nitrogen heterocycle. Compared with the existing corrosion inhibitors, it has more nitrogen functional groups, better adsorption effect, and can more effectively protect metals from corrosion.

[0033] Example 2

[0034] By changing the ratio of reactants (the molar ratio of citric acid to isoniazid is 2:1, 2:2, 2:3 respectively), synthesis temperature (140℃, 160℃, 180℃) and reaction time (4h, 6h, 8h), the corrosion inhibitor is prepared according to the above steps S1 to S5. The corrosion inhibition performance is measured by a static corrosion performance evaluation experiment. The specific experiment is as follows: the Q235 sample is immersed in a 4wt% NaCl aqueous solution, soaked for 48h, taken out, immersed in anhydrous ethanol for 30min to dehydrate, blown dry with cold air, rinsed, wiped the surface dry, and placed in an ultrasonic cleaner for 10min to remove surface corrosion products, then blown dry with cold air and weighed. According to the change in the weight of the sample, the corrosion inhibition efficiency of the corrosion inhibitor and the corrosion rate of the solution are calculated, as shown in formula (1)

[0035]

[0036] Where:

[0037] W o - Average weight of the specimens before corrosion, g;

[0038] W corr - Average weight of the sample after corrosion, g;

[0039] ρ-density of carbon steel, g / cm 3 ;

[0040] S- total area of ​​the sample, m 2 ;

[0041] T-immersion time, h.

[0042] The corrosion inhibition efficiency η was calculated according to formula (2) at different concentrations.

[0043]

[0044] Where:

[0045] v 0 -Corrosion rate value of the sample without corrosion inhibitor. mm / a;

[0046] v 1 -Corrosion rate value of the sample containing corrosion inhibitor. mm / a.

[0047] The corrosion inhibition effect is shown in Table 1 below.

[0048] Table 1:

[0049]

[0050] According to the corrosion inhibition efficiency, the preferred reaction molar ratio is 2:3, the reaction temperature is 160°C, and the reaction time is 6h.

[0051] Comparative Example

[0052] Weigh 0.38g of citric acid and 0.525g of citrulline respectively, with a molar ratio of 2:3, and prepare a nano corrosion inhibitor according to steps S2-S5 of Example 1. According to the corrosion inhibition performance test experiment in Example 1, the corrosion inhibition efficiency of the corrosion inhibitor is calculated using formula (2) in Example 1. The corrosion sample is low carbon steel, and the ambient temperature is controlled to be 30 degrees Celsius for 48 hours. The corrosion efficiency of the corrosion inhibitor is measured by the weight loss method. After experimental testing, the corrosion inhibition efficiency of the corrosion inhibitor prepared with citrulline as the nitrogen source is 67.5%, while the corrosion inhibition efficiency of the corrosion inhibitor prepared with isoniazid as the nitrogen source under the same conditions is as high as 85.5%, so isoniazid is selected as the nitrogen source material of the corrosion inhibitor.

[0053] Example 3

[0054] According to the steps S1-S5 of the above embodiment 1, a green nano corrosion inhibitor is prepared, and a 200 mg / L corrosion inhibitor aqueous solution is prepared. At the same time, a citric acid aqueous solution and an isoniazid aqueous solution of the same concentration are prepared. The corrosion sample selects low carbon steel, the corrosion solution is a 4wt% NaCl aqueous solution, and the added corrosion inhibitors are the prepared 200 mg / L corrosion inhibitor aqueous solution, citric acid aqueous solution and isoniazid aqueous solution. The ambient temperature is controlled to be 30 degrees Celsius and the time is 48h. The corrosion efficiency of the corrosion inhibitor is measured by the weight loss method. The corrosion efficiency of the corrosion inhibitor and the solution corrosion rate are calculated respectively using formula (1) and formula (2) in embodiment 1. In the above environment, the corrosion inhibition performance of the raw materials is 8.9% and 23.6%, respectively, which is much smaller than the corrosion inhibition efficiency of the synthetic corrosion inhibitor (88.2%), so the influence of the raw materials on the corrosion inhibition performance of the synthetic corrosion inhibitor can be ruled out.

[0055] Table 2

[0056]

[0057] Example 4

[0058] Two sets of parallel reagents were placed in a 4wt% NaCl solution at 30°C, and nano corrosion inhibitors with concentrations of 100ppm, 200ppm, 300ppm, 400ppm, 500ppm and 600ppm were added to the solution, respectively, and compared with the NaCl solution without corrosion inhibitor added as a blank control group. The sample was taken out after 40 hours, soaked in anhydrous ethanol for 30 minutes to dehydrate, dried with cold air, and rinsed. The surface was wiped dry and placed in an ultrasonic cleaner for 10 minutes to remove surface corrosion. After that, the weight was weighed after drying with cold air. According to the change in the weight of the sample, the corrosion efficiency of the corrosion inhibitor and the corrosion rate of the solution were calculated, as shown in formula (1)

[0059]

[0060] Where:

[0061] W o - Average weight of the specimens before corrosion, g;

[0062] W corr - Average weight of the sample after corrosion, g;

[0063] ρ-density of carbon steel, g / cm 3 ;

[0064] S- total area of ​​the sample, m 2 ;

[0065] T-immersion time, h.

[0066] The corrosion inhibition efficiency η was calculated according to formula (2) at different concentrations.

[0067]

[0068] Where:

[0069] v 0 -Corrosion rate value of the sample without corrosion inhibitor. mm / a;

[0070] v 1 -Corrosion rate value of the sample containing corrosion inhibitor. mm / a.

[0071] The static corrosion inhibition effect evaluation experiment of the samples with different concentrations of nano corrosion inhibitors was carried out, and the performance results are shown in Table 3. As shown in Table 3, in the static corrosion inhibition effect evaluation experiment, the nano corrosion inhibitor has good corrosion inhibition performance at 30°C (after 48h), and has a significant inhibitory effect on the NaCl solution corrosion of the sample. When the concentration of the corrosion inhibitor increases, the corrosion inhibition efficiency gradually increases. When the concentration of the corrosion inhibitor is 600ppm, the corrosion inhibition efficiency of the corrosion inhibitor reaches a maximum of 91.9%. However, when the concentration of the corrosion inhibitor exceeds 600ppm, the corrosion inhibition efficiency begins to decrease. It shows that the green nano corrosion inhibitor of the present invention has good resistance to NaCl solution corrosion.

[0072] Table 3

[0073]

Claims

1. A green and environmentally friendly nano-carbon dot corrosion inhibitor, characterized in that: Its structural formula is shown in formula (1):

2. The method for preparing the green and environmentally friendly nano-carbon dot corrosion inhibitor according to claim 1, characterized in that: Citric acid and isoniazid were used to synthesize nitrogen-doped carbon nanodots by hydrothermal synthesis, and the reaction flow is as follows:

3. The method for preparing the green and environmentally friendly nano-carbon dot corrosion inhibitor according to claim 2, characterized in that: Weigh citric acid and isoniazid, add deionized water to dissolve to obtain a mixed solution, transfer the mixed solution to a hydrothermal reactor, perform a hydrothermal reaction, and after the reaction, dialyze the obtained product in deionized water to obtain a carbon nanoparticle solution, dry it, and obtain nanocarbon dot corrosion inhibitor solid particles.

4. The method for preparing the green and environmentally friendly nano-carbon dot corrosion inhibitor according to claim 3, characterized in that: The molar ratio of citric acid to isoniazid is 2:1-3.

5. The method for preparing the green and environmentally friendly nano-carbon dot corrosion inhibitor according to claim 3, characterized in that: The hydrothermal reaction conditions are: 140-180°C for 4-8h.

6. The method for preparing the green and environmentally friendly nano-carbon dot corrosion inhibitor according to claim 3, characterized in that: The molar ratio of citric acid to isoniazid is 2:3; the hydrothermal reaction conditions are 160° C. for 6 hours.

7. The method for preparing the green and environmentally friendly nano-carbon dot corrosion inhibitor according to claim 3, characterized in that: The product was dialyzed in deionized water using a dialysis bag with a molecular weight of 1000 MD for 48 hours; the deionized water was changed every 4 hours.

8. Use of the green and environmentally friendly nano-carbon dot corrosion inhibitor according to claim 1 in metal corrosion protection.

Citation Information

Patent Citations

  • Citric acid-based functionalized carbon dot corrosion inhibitor and preparation method and application thereof

    CN111662243A

  • Green fluorescent carbon dot and preparation method and application thereof in rutin detection

    CN112608744A

  • A pickling agent method for in-situ preparation of nitrogen-doped carbon dot corrosion inhibitor

    CN114934273A

  • Nitrogen-doped carbon dot corrosion inhibitor for ground pipe network corrosion environment and preparation method of nitrogen-doped carbon dot corrosion inhibitor

    CN117963890A

  • Systems, compositions, and / or methods utilizing carbon dots

    WO2020112792A1