Preparation method of high-adsorptivity water-resistant honeycomb activated carbon

By using the combined technology of phosphate carbon and carboxymethyl cellulose and other materials, the problems of cracking and insufficient adsorption performance of honeycomb activated carbon during the production process are solved, and the preparation of honeycomb activated carbon with high adsorption and water resistance is achieved.

CN118851173AActive Publication Date: 2024-10-29NANPING YUANLI ACTIVE CARBON CO LTD

Patent Information

Application Number
CN202411115976.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-29
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

It is difficult to prepare high adsorption and water-resistant honeycomb activated carbon with the existing technology. Phosphate carbon is prone to cracking during the production process and has insufficient adsorption performance. Conventional methods lead to uneven drying and calcination of honeycomb carbon, which affects performance.

Method used

Using phosphate carbon as the base material, through carbonization, activation, phosphoric acid gradient recovery washing and high-temperature heat treatment, combined with carboxymethyl cellulose and silica sol, circulating hot air drying and medium-temperature calcination are used to reduce the cracking rate and improve the adsorption performance.

Benefits of technology

The iodine adsorption value and carbon tetrachloride adsorption rate of honeycomb carbon are significantly improved, the cracking rate and calcination shrinkage are reduced, and high adsorption and water resistance are achieved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of high-adsorbability water-resistant honeycomb activated carbon, which comprises the following steps: carrying out high-temperature heat treatment on a semi-finished product of phosphoric acid carbon activated at a relatively high temperature to prepare phosphoric acid carbon with high heat stability; the preparation method comprises the following steps: crushing the raw materials, mixing the crushed raw materials with attapulgite, carboxymethyl cellulose, a silica sol solution and the like according to a certain ratio, kneading, filtering, forming, drying in the shade, drying by a heat pump, and calcining at low temperature to obtain the high-adsorbability water-resistant honeycomb carbon. Phosphoric acid carbon is adopted as base carbon, micropores are developed compared with physical carbon, and the honeycomb carbon prepared from the phosphoric acid carbon is higher in adsorption performance. And performing high-temperature heat treatment on the semi-finished product of the phosphoric acid charcoal activated at a relatively high temperature to obtain the phosphoric acid charcoal with high heat stability. A proper amount of carboxymethyl cellulose and silica sol are added in the honeycomb carbon manufacturing process, and the cracking rate of honeycomb carbon during drying and calcination is reduced. Circulating hot air is adopted for heat supply in the drying process, heating is uniform, the drying cracking rate is reduced, and the drying time is shortened. Medium-temperature calcination is adopted, so that the shrinkage rate and the cracking rate of the honeycomb carbon in the calcination process are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental protection, and in particular to a method for preparing highly adsorbable and water-resistant honeycomb activated carbon. Background Art

[0002] Due to the particularity of its activation mechanism, phosphate carbon has a high yield in the production process. Its micropores are higher than those of conventional physical carbon, and it has a higher iodine adsorption value and carbon tetrachloride adsorption rate. However, conventional phosphate carbon has a low specific gravity, and because its activation temperature is only 380-450°C, it is easy to crack during the process of making honeycomb carbon, especially during the calcination process. In addition, the surface of phosphate carbon contains a large number of acidic groups, which makes it have poor affinity with the clay used to prepare honeycomb carbon. Based on these characteristics, conventional phosphate carbon is difficult to be used as a raw material for preparing honeycomb carbon.

[0003] Most honeycomb charcoals on the market are made of coal-based charcoal and clay, which are then heated and dried conventionally, and then calcined at a high temperature of more than 700°C to prepare water-resistant honeycomb charcoal. Coal-based charcoal itself has poor adsorption properties, and it is difficult to prepare honeycomb charcoal with high iodine adsorption value and high carbon tetrachloride adsorption rate. The conventional heating and drying method causes uneven heating and easy cracking. In order to prevent cracking, it needs to be dried for a long time of 5-6 days; and during the high-temperature calcination process, the honeycomb charcoal has a high shrinkage rate and a high cracking rate. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a method for preparing highly adsorbable and water-resistant honeycomb activated carbon.

[0005] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:

[0006] A method for preparing highly adsorbable and water-resistant honeycomb activated carbon, comprising:

[0007] S1, screening wood and bamboo chips according to 3-12 mesh components, and mixing them with phosphoric acid according to a first preset ratio to obtain a first mixture;

[0008] S2, carbonizing and reactivating the first mixed material to obtain a phosphate carbon activated material;

[0009] S3, washing and drying the activated carbon phosphate material with a phosphoric acid gradient recovery method to obtain a carbon phosphate semi-finished product;

[0010] S4, placing the semi-finished carbon phosphate product in an externally heated converter into which an inert gas is introduced, and grinding the product after high-temperature heat treatment to obtain carbon phosphate;

[0011] S5, mixing carbon phosphate, attapulgite and carboxymethyl cellulose according to a second preset ratio, adding a silica sol solution of a preset concentration and kneading for 20 to 30 minutes to obtain a second mixture;

[0012] S6, adding engine oil to the second mixed material, kneading for 10 to 30 minutes, and obtaining a honeycomb carbon kneaded material;

[0013] S7, placing the honeycomb carbon kneaded material in a rough smelting machine for rough smelting to obtain a cylindrical slurry, then conveying the cylindrical slurry to a filter for filtering, and conveying the filtered cylindrical slurry to a refining smelting machine for multiple refining to obtain a cylindrical slurry;

[0014] S8, transporting the cylindrical mud material to an extrusion molding machine for extrusion molding to obtain a honeycomb wet blank;

[0015] S9, transporting the honeycomb wet blank to a shade drying room for shade drying to obtain a honeycomb shaped blank;

[0016] S10, transporting the honeycomb shaped blank to a drying room, slowly heating it up according to a preset temperature gradient using circulating hot air, to obtain a honeycomb dry blank with a moisture content of less than 5%;

[0017] S11. Place the honeycomb dry blank in an oxygen-free calcining furnace, slowly heat it to the calcining temperature and keep it warm, and wait for it to cool naturally to room temperature to obtain honeycomb activated carbon.

[0018] In some embodiments, in step S1, the first preset ratio ranges from 1:1.4 to 1:1.8, phosphoric acid is obtained from a phosphoric acid solution, and the phosphoric acid concentration in the phosphoric acid solution is 50% to 80%.

[0019] In some embodiments, step S2 further includes:

[0020] The first mixed material is kept at a carbonization temperature range of 250-350° C. for 20-60 minutes to obtain a carbonized mixed material;

[0021] The carbonized mixture is kept at an activation temperature range of 500-600° C. for 10-30 minutes to obtain a phosphate carbon activated material.

[0022] In some embodiments, step S3 further includes:

[0023] The activated phosphate carbon material is washed until the pH of the carbon is ≥ 2.5, and the activated phosphate carbon material is dried until the moisture content is ≤ 10%.

[0024] In some embodiments, step S4 further includes:

[0025] Nitrogen is introduced into the externally heated converter, and the temperature of the externally heated converter is maintained at 500-650° C. for 0.5-1.5 hours. The particle size of the ground powder is set to 200 meshes, and the passing rate is ≤5%.

[0026] In some embodiments, step S5 further includes:

[0027] Mixing carbon phosphate, attapulgite and carboxymethyl cellulose in a ratio of 100 parts of carbon phosphate, 40-60 parts of attapulgite and 0.5-1.5 parts of carboxymethyl cellulose, and adding 110-120 parts of silica sol solution, wherein the preset concentration range is 1-2%;

[0028] Step S6 also includes:

[0029] Add 1 part of engine oil to the second mixture, the engine oil is gear oil.

[0030] In some embodiments, step S7 further includes:

[0031] The cylindrical mud material is transported to a filter with a screen of 40-60 mesh for filtration, and is refined multiple times in a mud refining machine with a vacuum degree of 0.08-0.1 MPa, and the number of times of mud refining is 1-3 times.

[0032] In some embodiments, step S9 further includes:

[0033] The wet honeycomb blanks are transported to a shade drying room with a temperature of 20-25° C. and a relative humidity of 50-70% for shade drying for 2-3 days.

[0034] In some embodiments, step S10 further includes:

[0035] The circulating hot air in the drying room is provided by two heat pumps;

[0036] The drying conditions of the drying room are set to a temperature of 30-40° C. and a relative humidity of 85-95%, and the honeycomb-shaped blank is placed in the drying room for primary drying for 24 hours to obtain a primary dried blank;

[0037] The drying conditions in the drying room are set to a temperature of 40-50° C. and a relative humidity of 70-85%, and the primary dried blank is placed in the drying room for secondary drying for 24 hours to obtain a secondary dried blank;

[0038] The drying conditions of the drying room are set to a temperature of 50-60° C. and a relative humidity of 50-70%, and the secondary dried blank is placed in the drying room for tertiary drying for 24 hours to obtain a tertiary dried blank, which is recorded as a honeycomb dry blank.

[0039] In some embodiments, step S11 further includes:

[0040] The oxygen-free calcining furnace is controlled to slowly heat up to a calcining temperature of 500-550°C within 7-9 hours, and kept warm for 1-3 hours.

[0041] By adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0042] (1) Phosphate carbon is used as the base carbon. Due to the particularity of its activation mechanism, the mesopores of phosphate carbon are more developed than those of physical carbon. The iodine adsorption value of the honeycomb carbon prepared can be greater than 800 mg / g, and the carbon tetrachloride adsorption rate can be greater than 70%.

[0043] (2) The phosphate carbon is activated at a higher temperature than conventional phosphate carbon, and then acid recovered, washed, and dried. The resulting phosphate carbon semi-finished product is subjected to high-temperature heat treatment, which can significantly improve the thermal stability of the phosphate carbon and reduce the surface acidic groups of the phosphate carbon, making it less likely to shrink or crack during the production of honeycomb carbon.

[0044] (3) Add appropriate amount of carboxymethyl cellulose and silica sol during the production process of honeycomb charcoal to reduce the cracking rate of honeycomb charcoal during drying and calcination.

[0045] (4) The drying process of honeycomb charcoal uses circulating hot air generated by two heat pumps to provide heating, so that the honeycomb charcoal in the drying room is heated evenly, reducing the cracking rate during the drying process and shortening the drying time.

[0046] (5) Honeycomb charcoal is calcined at a medium temperature of 500-550°C. This calcination temperature is more suitable for honeycomb charcoal made from phosphate carbon, which reduces the shrinkage and cracking rate of honeycomb charcoal during the calcination process. DETAILED DESCRIPTION

[0047] The present invention will be further described in detail below in conjunction with the embodiments. It is particularly noted that the following embodiments are only used to illustrate the present invention, but are not intended to limit the scope of the present invention. Similarly, the following embodiments are only partial embodiments of the present invention rather than all embodiments, and all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.

[0048] A method for preparing highly adsorbable and water-resistant honeycomb activated carbon, comprising:

[0049] S1, screening wood and bamboo chips according to 3-12 mesh components, and mixing them with phosphoric acid according to a first preset ratio to obtain a first mixture;

[0050] S2, carbonizing and activating the first mixed material to obtain activated phosphate carbon material;

[0051] S3, washing and drying the activated carbon phosphate material with a phosphoric acid gradient recovery method to obtain a carbon phosphate semi-finished product;

[0052] S4, placing the semi-finished carbon phosphate product in an externally heated converter into which an inert gas is introduced, and grinding the product after high-temperature heat treatment to obtain carbon phosphate;

[0053] S5, mixing carbon phosphate, attapulgite and carboxymethyl cellulose according to a second preset ratio, adding a silica sol solution of a preset concentration and kneading for 20 minutes to obtain a second mixture;

[0054] S6, adding engine oil to the second mixed material, kneading for 10 minutes, and obtaining a honeycomb carbon kneaded material;

[0055] S7, placing the honeycomb carbon kneaded material in a rough smelting machine for rough smelting to obtain a cylindrical slurry, then conveying the cylindrical slurry to a filter for filtering, and conveying the filtered cylindrical slurry to a refining smelting machine for multiple refining to obtain a cylindrical slurry;

[0056] S8, transporting the cylindrical mud material to an extrusion molding machine for extrusion molding to obtain a honeycomb wet blank;

[0057] S9, transporting the honeycomb wet blank to a shade drying room for shade drying to obtain a honeycomb shaped blank;

[0058] S10, transporting the honeycomb shaped blank to a drying room, slowly heating it up according to a preset temperature gradient using circulating hot air, to obtain a honeycomb dry blank with a moisture content of less than 5%;

[0059] S11. Place the honeycomb dry blank in an oxygen-free calcining furnace, slowly heat it to the calcining temperature and keep it warm, and wait for it to cool naturally to room temperature to obtain honeycomb activated carbon.

[0060] In some embodiments, in step S1, the first preset ratio ranges from 1:1.4 to 1:1.8, phosphoric acid is obtained from a phosphoric acid solution, and the phosphoric acid concentration in the phosphoric acid solution is 50% to 80%.

[0061] In some embodiments, step S2 further includes:

[0062] The first mixed material is kept at a carbonization temperature range of 250-350° C. for 20-60 minutes to obtain a carbonized mixed material;

[0063] The carbonized mixture is kept at an activation temperature range of 500-600° C. for 10-20 minutes to obtain a phosphate carbon activated material.

[0064] In some embodiments, step S3 further includes:

[0065] The activated phosphate carbon material is washed until the pH of the carbon is ≥ 2.5, and the activated phosphate carbon material is dried until the moisture content is ≤ 10%.

[0066] In some embodiments, step S4 further includes:

[0067] Nitrogen is introduced into the externally heated converter, and the temperature of the externally heated converter is maintained at 500-650° C. for 0.5-1.5 hours. The particle size of the ground powder is set to 200 meshes, and the passing rate is ≤5%.

[0068] In some embodiments, step S5 further includes:

[0069] Mixing carbon phosphate, attapulgite and carboxymethyl cellulose in a ratio of 100 parts of carbon phosphate, 40-60 parts of attapulgite and 0.5-1.5 parts of carboxymethyl cellulose, and adding 110-120 parts of silica sol solution, wherein the preset concentration range is 1-2%;

[0070] Step S6 also includes:

[0071] Add 1 part of engine oil to the second mixture, the engine oil is gear oil.

[0072] In some embodiments, step S7 further includes:

[0073] The cylindrical mud material is transported to a filter with a screen of 40-60 mesh for filtration, and is refined multiple times in a mud refining machine with a vacuum degree of 0.08-0.1 MPa, and the number of times of mud refining is 1-3 times.

[0074] In some embodiments, step S9 further includes:

[0075] The wet honeycomb blanks are transported to a shade drying room with a temperature of 20-25° C. and a relative humidity of 50-70% for shade drying for 2-3 days.

[0076] In some embodiments, step S10 further includes:

[0077] The circulating hot air in the drying room is provided by two heat pumps;

[0078] The drying conditions in the drying room are set to a temperature of 30-40° C. and a relative humidity of 85-95%, and the honeycomb-shaped blank is placed in the drying room for primary drying for 24 hours to obtain a primary dried blank;

[0079] The drying conditions in the drying room are set to a temperature of 40-50° C. and a relative humidity of 70-85%, and the primary dried blank is placed in the drying room for secondary drying for 24 hours to obtain a secondary dried blank;

[0080] The drying conditions of the drying room are set to a temperature of 50-60° C. and a relative humidity of 50-70%, and the secondary dried blank is placed in the drying room for tertiary drying for 24 hours to obtain a tertiary dried blank, which is recorded as a honeycomb dry blank.

[0081] In some embodiments, step S11 further includes:

[0082] The oxygen-free calcining furnace is controlled to slowly heat up to a calcining temperature of 500-550°C within 7-9 hours, and kept warm for 1-3 hours.

[0083] Embodiment 1:

[0084] Preparation of carbon phosphate:

[0085] (1) screening wood and bamboo chips, taking out 3-12 mesh fractions, and mixing them with 50-80% phosphoric acid in a ratio of 1:1.4-1:1.8 of wood and bamboo chips to pure phosphoric acid to obtain a first mixture;

[0086] (2) The first mixed material is heated to a carbonization temperature of 250-350° C., kept warm for 20-60 minutes, and then heated to an activation temperature of 500-600° C., kept warm for 10-20 minutes, to obtain an activated phosphate carbon material.

[0087] (3) washing the activated phosphate carbon material with phosphoric acid gradient recovery until the pH of the carbon is ≥ 2.5, and drying the activated phosphate carbon material until the moisture content is ≤ 10% to prepare a phosphate carbon semi-finished product;

[0088] (4) The semi-finished phosphate carbon is heated to a heat treatment temperature of 500-650°C in an externally heated converter under a nitrogen atmosphere and kept at this temperature for 0.5-1.5 hours. The particle size of the re-grinded powder is controlled to have a passing rate of 200 meshes ≤5%. Phosphate carbon is obtained.

[0089] Preparation of honeycomb charcoal:

[0090] (5) Mixing and kneading: After mixing 100 parts of phosphate carbon, 40-60 parts of attapulgite, and 0.5-1.5 parts of carboxymethyl cellulose, add 110-120 parts of 1-2% silica sol solution, knead for 20 minutes, then add 1 part of gear oil, and knead for 10 minutes to obtain a honeycomb carbon kneaded material.

[0091] (6) Mud kneading and molding: The honeycomb carbon kneaded material is roughly kneaded by a rough mud kneading machine to obtain a cylindrical mud material, and then the impurities are filtered out by a filter with a 40-60 mesh screen. After filtration, the mud material passes through a fine mud kneading machine with a vacuum degree of 0.08-0.1MPa for 1-3 times to obtain a smooth and compact cylindrical mud material. Finally, the cylindrical mud material is transported to an extrusion molding machine with a honeycomb mold for extrusion molding to obtain a honeycomb wet blank.

[0092] (7) Drying in the shade: The wet honeycomb material is placed in a shade drying room at a temperature of 20-25° C. and a relative humidity of 50-70% for 2-3 days to allow it to slowly lose moisture and solidify, thereby obtaining a honeycomb shaped blank.

[0093] (8) Heat pump rapid drying: The honeycomb shaped material is transported to a drying room equipped with two heat pumps and dried at 30-40° C. and a relative humidity of 85-95% for 1 day under circulating hot air heating; the temperature is raised to 40-50° C. and a relative humidity of 70-85% for 1 day; the temperature is then raised to 50-60° C. and a relative humidity of 50-70% for 1 day. The moisture content after drying is less than 5%, thereby obtaining a honeycomb dry blank material.

[0094] (9) Medium-temperature calcination: The honeycomb dry material is placed in a sealed oxygen-deficient calcining furnace and slowly heated to a calcination temperature of 500-550°C over 7-9 hours. The calcination is completed after keeping the temperature for 1-3 hours. The calcination furnace is then cooled naturally to room temperature to obtain honeycomb activated carbon.

[0095] Embodiment 2:

[0096] Preparation of carbon phosphate:

[0097] (1) screening wood and bamboo chips, taking out the 3-12 mesh fraction, and mixing it with 70% phosphoric acid in a ratio of 1:1.6 between wood and bamboo chips and pure phosphoric acid to obtain a first mixture;

[0098] (2) The first mixed material is heated to a carbonization temperature of 300°C, kept at this temperature for 40 minutes, and then heated to an activation temperature of 550°C, kept at this temperature for 15 minutes to obtain an activated phosphate carbon material.

[0099] (3) The activated phosphate carbon material is washed with phosphoric acid gradient recovery to a carbon pH of ≥2.5, and then dried to a moisture content of ≤10% to prepare a phosphate carbon semi-finished product;

[0100] (4) The semi-finished phosphate carbon is heated to a heat treatment temperature of 600°C in an externally heated converter under a nitrogen atmosphere and kept at this temperature for 1 hour. The particle size of the re-grinded powder is controlled to have a passing rate of 200 meshes ≤5%. Phosphate carbon is obtained.

[0101] Preparation of honeycomb charcoal:

[0102] (5) Mixing and kneading: 100 parts of phosphate carbon, 50 parts of attapulgite, and 1 part of carboxymethyl cellulose were mixed, and 115 parts of 1.5% silica sol solution were added. After kneading for 20 minutes, 1 part of gear oil was added and kneaded for 10 minutes to obtain a honeycomb carbon kneaded material.

[0103] (6) Mud kneading and molding: The honeycomb carbon kneaded material is roughly kneaded by a rough mud kneading machine to obtain a cylindrical mud material, and then the impurities are filtered out by a filter with a 50-mesh screen. After filtering, the mud material is refined twice by a fine mud kneading machine with a vacuum degree of 0.08-0.1MPa to obtain a smooth and compact cylindrical mud material. Finally, the cylindrical mud material is transported to an extrusion molding machine with a honeycomb mold for extrusion molding to obtain a honeycomb wet blank.

[0104] (7) Drying in the shade: The wet honeycomb material is placed in a shade drying room at a temperature of 20-25° C. and a relative humidity of 50-70% for 2.5 days to allow it to slowly lose moisture and solidify, thereby obtaining a honeycomb shaped blank.

[0105] (8) Heat pump rapid drying: The honeycomb shaped material is transported to a drying room equipped with two heat pumps and dried at 30-40° C. and a relative humidity of 85-95% for 1 day under circulating hot air heating; the temperature is raised to 40-50° C. and a relative humidity of 70-85% for 1 day; the temperature is then raised to 50-60° C. and a relative humidity of 50-70% for 1 day. The moisture content after drying is less than 5%, thereby obtaining a honeycomb dry blank material.

[0106] (9) Medium-temperature calcination: The honeycomb dry material is placed in a sealed oxygen-deficient calcining furnace and slowly heated to a calcining temperature of 525°C over 8 hours. The calcination is completed after keeping the temperature for 2 hours. The calcining furnace is cooled naturally to room temperature to obtain honeycomb activated carbon.

[0107] The above technical solution has the following advantages:

[0108] (1) Phosphate carbon is used as the base carbon. Due to the particularity of its activation mechanism, the mesopores of phosphate carbon are more developed than those of physical carbon. The iodine adsorption value of the honeycomb carbon obtained (test standard: GB / T 12496.8-2015 "Test method for wood activated carbon - Determination of iodine adsorption value") can be greater than 800 mg / g, and the carbon tetrachloride adsorption rate (test standard: GB / T 12496.5-1999 "Test method for wood activated carbon - Determination of carbon tetrachloride adsorption rate (activity)") can be greater than 70%.

[0109] (2) The phosphate carbon semi-finished product is activated at a higher temperature than conventional phosphate carbon, and then subjected to high-temperature heat treatment to improve the thermal stability of the phosphate carbon. At the same time, the high-temperature heat treatment of the phosphate carbon semi-finished product can also reduce the surface acidic groups of the phosphate carbon, making it less likely to shrink and crack during the production of honeycomb carbon.

[0110] (3) Add appropriate amount of carboxymethyl cellulose and silica sol during the production process of honeycomb charcoal to reduce the cracking rate of honeycomb charcoal during drying and calcination.

[0111] (4) The drying process of honeycomb charcoal uses circulating hot air generated by two heat pumps to provide heating, so that the honeycomb charcoal in the drying room is heated evenly, reducing the cracking rate during the drying process and shortening the drying time.

[0112] (5) Honeycomb charcoal is calcined at a medium temperature of 500-550°C. This calcination temperature is more suitable for honeycomb charcoal made from phosphate carbon, which reduces the shrinkage and cracking rate of honeycomb charcoal during the calcination process.

[0113] The above descriptions are only some embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Any equivalent device or equivalent process transformation made using the specification of the present invention, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing highly adsorbable water-resistant honeycomb activated carbon, characterized in that: include: S1, screening wood and bamboo chips according to 3-12 mesh components, and mixing them with phosphoric acid according to a first preset ratio to obtain a first mixture; S2, carbonizing and reactivating the first mixed material to obtain a phosphate carbon activated material; S3, performing gradient recovery washing of phosphoric acid on the activated carbon phosphate material and drying the same to obtain a carbon phosphate semi-finished product; S4, placing the semi-finished carbon phosphate product in an externally heated converter into which an inert gas is introduced, and grinding the semi-finished carbon phosphate product after high-temperature heat treatment to obtain carbon phosphate; S5, mixing carbon phosphate, attapulgite and carboxymethyl cellulose according to a second preset ratio, adding a silica sol solution of a preset concentration and kneading for 20 to 30 minutes to obtain a second mixture; S6, adding engine oil to the second mixed material, kneading for 10 to 30 minutes, to obtain a honeycomb carbon kneaded material; S7, placing the honeycomb carbon kneaded material in a rough smelting machine for rough smelting to obtain a cylindrical slurry, then conveying the cylindrical slurry to a filter for filtering, and conveying the filtered cylindrical slurry to a fine smelting machine for multiple fine smelting to obtain a cylindrical slurry; S8, transporting the cylindrical mud material to an extrusion molding machine for extrusion molding to obtain a honeycomb wet blank; S9, transporting the honeycomb wet blank to a shade drying room for shade drying to obtain a honeycomb shaped blank; S10, transporting the honeycomb shaped blank to a drying room, slowly heating it with circulating hot air according to a preset temperature gradient to obtain a honeycomb dry blank with a moisture content of less than 5%; S11, placing the honeycomb dry blank in an oxygen-free calcining furnace, slowly heating it to a calcining temperature and keeping it warm, waiting for it to cool naturally to room temperature, and obtaining honeycomb activated carbon.

2. The method for preparing highly adsorbable water-resistant honeycomb activated carbon according to claim 1, characterized in that: In step S1, the first preset ratio has a value range of 1:1.4-1:1.8, the phosphoric acid is obtained from a phosphoric acid solution, and the phosphoric acid concentration in the phosphoric acid solution is 50%-80%.

3. The method for preparing highly adsorbable water-resistant honeycomb activated carbon according to claim 1, characterized in that: Step S2 also includes: The first mixed material is kept at a carbonization temperature range of 250-350° C. for 20-60 minutes to obtain a carbonized mixed material; The carbonized mixed material is kept at an activation temperature range of 500-600° C. for 10-30 minutes to obtain a phosphate carbon activated material.

4. The method for preparing highly adsorbable water-resistant honeycomb activated carbon according to claim 1, characterized in that: Step S3 also includes: The activated phosphate carbon material is washed until the pH of the carbon is ≥2.5, and the activated phosphate carbon material is dried until the moisture content is ≤10%.

5. The method for preparing highly adsorbable water-resistant honeycomb activated carbon according to claim 1, characterized in that: Step S4 also includes: Nitrogen is introduced into the externally heated converter, and the temperature of the externally heated converter is maintained at 500-650° C. for 0.5-1.5 hours. The particle size of the ground powder is set to 200 meshes, and the passing rate is ≤5%.

6. The method for preparing highly adsorbable water-resistant honeycomb activated carbon according to claim 1, characterized in that: Step S5 also includes: Mixing carbon phosphate, attapulgite and carboxymethyl cellulose in a ratio of 100 parts of carbon phosphate, 40-60 parts of attapulgite and 0.5-1.5 parts of carboxymethyl cellulose, and adding 110-120 parts of silica sol solution, wherein the preset concentration ranges from 1% to 2%; Step S6 also includes: Add 1 part of engine oil to the second mixture, the engine oil is gear oil.

7. The method for preparing highly adsorbable water-resistant honeycomb activated carbon according to claim 1, characterized in that: The step S7 further comprises: The cylindrical mud material is conveyed to a filter with a screen of 40-60 meshes for filtration, and is refined for multiple times in a mud refiner with a vacuum degree of 0.08-0.1 MPa, the number of times of mud refinement is 1-3 times.

8. The method for preparing highly adsorbable water-resistant honeycomb activated carbon according to claim 1, characterized in that: The step S9 further comprises: The wet honeycomb blank is transported to a shade drying room with a temperature of 20-25° C. and a relative humidity of 50-70% for shade drying for 2-3 days.

9. The method for preparing highly adsorbable water-resistant honeycomb activated carbon according to claim 1, characterized in that: The step S10 further includes: The circulating hot air in the drying room is provided by two heat pumps; The drying conditions of the drying room are set to a temperature of 30-40° C. and a relative humidity of 85-95%, and the honeycomb shaped blank is placed in the drying room for primary drying for 24 hours to obtain a primary dried blank; The drying conditions of the drying room are set to a temperature of 40-50° C. and a relative humidity of 70-85%, and the primary dried blank is placed in the drying room for secondary drying for 24 hours to obtain a secondary dried blank; The drying conditions of the drying room are set to a temperature of 50-60° C. and a relative humidity of 50-70%, and the secondary dried blank is placed in the drying room for tertiary drying for 24 hours to obtain a tertiary dried blank, which is recorded as the honeycomb dry blank.

10. The method for preparing highly adsorbable water-resistant honeycomb activated carbon according to claim 1, characterized in that: The step S11 further includes: The oxygen-free calcining furnace is controlled to slowly heat up to a calcining temperature of 500-550° C. within 7-9 hours, and the temperature is kept for 1-3 hours.

Citation Information

Patent Citations

  • Preparation method of phenolic resin combined honeycomb activated carbon

    CN101857224A

  • Method for preparing activated carbon by taking walnut shells as raw materials

    CN109319779A

  • Activated carbon, raw material and green body for preparing activated carbon, and preparation method of green body

    CN115557498A

  • Production method of self-adhesive high-strength wooden columnar activated carbon

    CN115818642A

  • Production method of water-resistant honeycomb activated carbon

    CN116239118A

Cited By

  • Porous spongy honeycomb carbon material and preparation method thereof

    CN121318532A