Silicon-oxygen composite material as well as preparation method and application thereof
The reduced graphene oxide-coated silicon oxygen gel material was prepared through a redox self-assembly method, which solved the problems of volume expansion and poor conductivity of silicon anode materials during charging and discharging, and improved battery performance.
Patent Information
- Application Number
- CN202410848836.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
AI Technical Summary
Silicon anode materials suffer from severe volume expansion and poor conductivity during the charge and discharge process, resulting in poor cycle performance and rate performance, and cannot meet the needs of electric vehicles and energy storage fields.
The reduced graphene oxide-coated silicon-oxygen gel material is prepared through a redox self-assembly method, and is calcined to obtain a three-dimensional porous silicon-oxygen composite material, which reserves expansion space and improves electrical conductivity.
It significantly improves the first efficiency, rate performance and cycle stability of the battery, alleviates the volume expansion problem of silicon-oxygen materials during charge and discharge, and improves the transmission efficiency of lithium ions.
Smart Images

Figure CN118851184A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries and relates to a silicon-oxygen composite material and a preparation method and application thereof. Background Art
[0002] With the rapid development of electric vehicles and energy storage, the low theoretical capacity (372mAh / g) of traditional graphite negative electrode materials can no longer meet people's needs. Silicon negative electrode materials have the advantages of high theoretical specific capacity (4200mAh / g), environmental friendliness, low voltage platform and abundant resources. However, silicon has serious volume expansion (>300%) during the charging and discharging process, which will cause the electrode material to rupture and even pulverize, resulting in extremely poor cycle performance. At the same time, its own poor conductivity will also restrict its development.
[0003] The study found that SiO x (Silicon oxide, theoretical specific capacity ~2043mAh / g) has relatively good cycle stability. The lithium salt and lithium oxide produced during the first charge and discharge process can prevent the agglomeration of silicon particles and buffer their volume expansion during the charge and discharge process. For example, CN 117878236A discloses a preparation method and application of silicon-oxygen negative electrode materials. The method comprises the following steps: vapor-depositing silicon powder and silicon dioxide under vacuum to form SiO x A composite material cluster, wherein 0<x≤2, is a silicon-oxygen negative electrode material. The silicon-oxygen negative electrode material has a high charge-discharge specific capacity and a stable cycle property. The preparation method of the silicon-oxygen negative electrode material has a simple process, low cost, and a high yield of experimental materials, and can achieve large-scale mass production.
[0004] However, silicon oxide still has a large volume expansion (>200%) during the process of lithium insertion and extraction, which leads to the continuous formation of thicker SEI film and new solid interface, resulting in lower first efficiency and cycle performance. At the same time, its lower conductivity also leads to lower rate performance of the battery.
[0005] Based on the above research, it is necessary to provide a method for preparing a silicon-oxygen composite material. The material obtained by the preparation method has expansion space and excellent conductivity, and can improve the first efficiency, rate performance and cycle stability of the battery. Summary of the invention
[0006] The purpose of the present invention is to provide a silicon-oxygen composite material and a preparation method and application thereof. The preparation method can obtain a silicon-oxygen gel material coated with reduced graphene oxide through redox self-assembly, and finally obtain a three-dimensional porous silicon-oxygen composite material through calcination, which reserves space for the expansion of the silicon-oxygen material and improves the conductivity of the material, thereby improving the first efficiency, rate performance and cycle stability of the battery.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing a silicon-oxygen composite material, the preparation method comprising the following steps:
[0009] (1) mixing carboxylated graphene oxide, an amino silicon source and a solvent, performing solid-liquid separation and drying to obtain a precursor material;
[0010] (2) mixing and reacting the precursor material, reducing agent and solvent described in step (1), and then drying to obtain an aerogel material;
[0011] (3) calcining the aerogel material of step (2) to obtain the silicon-oxygen composite material.
[0012] The present invention first utilizes the carboxyl groups on the surface of graphene oxide to condense with the aminoamide on the surface of the amino silicon source to generate a graphene oxide-coated precursor, such as a graphene oxide-coated silicon dioxide (GO@SiO2) precursor; then, an aerogel material coated with reduced graphene oxide is prepared by a redox self-assembly hydrothermal method, such as a reduced graphene oxide-coated silicon dioxide (rGO@SiO2) aerogel; finally, a three-dimensional porous silicon-oxygen material coated with reduced graphene oxide is prepared by high-temperature calcination, such as a reduced graphene oxide-coated silicon dioxide (rGO@SiO2) aerogel. x ) composite negative electrode material.
[0013] The silicon-oxygen composite material prepared by the present invention has a core-shell structure coated with reduced graphene oxide, and the outer reduced graphene oxide shell can not only improve the conductivity of the silicon-oxygen material, but also inhibit the excessive volume expansion of silicon during the charge and discharge process, thereby improving the first efficiency, rate performance and cycle stability of the battery; at the same time, the silicon-oxygen composite material of the present invention has a three-dimensional network structure, which reserves expansion space for the internal stress caused by the volume expansion and contraction of the silicon-oxygen material during the charge and discharge process, further improving the cycle stability, and the three-dimensional network structure is conducive to the transmission of lithium ions, further improving the electrochemical performance of the battery.
[0014] Preferably, the particle size D50 of the amino silicon source in step (1) is 0.1-5 μm, for example, 0.1 μm, 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm or 5 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] The particle size of the amide silicon source of the present invention will affect the material properties. If the particle size D50 of the amide silicon source is too small, it will easily lead to agglomeration. If the particle size D50 of the amide silicon source is too large, it will be unfavorable for graphite coating.
[0016] Preferably, the amide silicon source in step (1) comprises amide silicon dioxide.
[0017] The present invention uses amino silicon dioxide as a raw material, which has the advantage of avoiding the generation of silicon dioxide in the process and the product compared with directly using amino silicon oxide.
[0018] The preparation method of the amino silicon dioxide of the present invention comprises the following steps: activating nano silicon dioxide powder at 110° C. for 2 hours and then dispersing the powder into toluene, adding KH5505 which is 10% of the mass of silicon dioxide, reacting the powder at 70° C. for 6 hours, cooling the powder to room temperature after the reaction is completed, centrifuging, washing and freeze-drying the powder to obtain the amino silicon dioxide.
[0019] Preferably, the mass ratio of the carboxylated graphene oxide and the amino silicon source in step (1) is (0.1-1):10, for example, it can be 0.1:10, 0.25:10, 0.5:10, 0.75:10 or 1:10, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the method for preparing the carboxylated graphene oxide in step (1) comprises: mixing a dispersion of carbodiimide hydrochloride, an imide compound and graphene oxide.
[0021] Preferably, the carbodiimide hydrochloride comprises 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride.
[0022] Preferably, the imide compound includes N-hydroxysuccinimide.
[0023] The invention adopts 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide to activate the carboxyl group.
[0024] Preferably, washing is performed between the solid-liquid separation and drying in step (1), and the washing liquid used for the washing comprises water and methanol.
[0025] Preferably, the drying method in step (1) includes freeze-drying.
[0026] The graphene oxide obtained in step (1) of the present invention is coated with silicon dioxide, and the graphene oxide may contain one or more silicon dioxide particles.
[0027] Preferably, the reaction temperature in step (2) is 90-180°C, for example, 90°C, 100°C, 120°C, 140°C, 160°C or 180°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable, preferably 120-180°C.
[0028] The reaction temperature of step (2) of the present invention will affect the reaction effect. If the reaction temperature is too low, a three-dimensional gel structure cannot be formed. If the reaction temperature is too high, the three-dimensional gel formed has small pores and a solid gel, which is not conducive to the transmission of ions.
[0029] Preferably, the reaction time of step (2) is 1.5-6 h, for example, 1.5 h, 2 h, 4 h or 6 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] The reaction of the present invention is carried out in a stainless steel autoclave lined with Teflon and is a hydrothermal reaction.
[0031] Preferably, in the mixed solution obtained by mixing in step (2), the concentration of the precursor material is 2.5-6 mg / mL, for example, it can be 2.5 mg / mL, 3 mg / mL, 4 mg / mL, 5 mg / mL or 6 mg / mL, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0032] In the present invention, the precursor material obtained in step (1) is preferably first ultrasonically dispersed in deionized water to obtain a solution with a concentration of 2.5-6 mg / mL of the precursor material, and then a reducing agent is added.
[0033] Preferably, the drying method in step (2) includes freeze-drying.
[0034] Preferably, after the reaction in step (2), impurities are first removed and then dried.
[0035] Preferably, the impurity removal method includes immersing in water and an alcohol solvent for dialysis removal, and the alcohol solvent is ethanol.
[0036] Preferably, the mass ratio of the precursor material and the reducing agent in step (2) is (0.2-2.5):1, for example, it can be 0.2:1, 0.5:1, 1:1, 1.5:1, 2:1 or 2.5:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, the reducing agent in step (2) comprises any one of sodium bisulphite formaldehyde, sodium sulfide, ascorbic acid, hydrogen iodide or hydroquinone, or a combination of at least two thereof.
[0038] Preferably, the calcination temperature in step (3) is 900-1100°C, for example, 900°C, 1000°C, or 1100°C, and the calcination time is 2-4h, for example, 2h, 3h or 4h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0039] Preferably, the calcination in step (3) is carried out under a protective atmosphere.
[0040] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps:
[0041] (1) mixing a dispersion of carbodiimide hydrochloride, an imide compound and graphene oxide, then adding an amide silicon source to the mixed solution and continuing to mix, and then performing solid-liquid separation, washing and freeze-drying to obtain a precursor material;
[0042] The amino silicon source is amino silicon dioxide with a particle size D50 of 0.1-5 μm;
[0043] (2) mixing the precursor material, reducing agent and solvent described in step (1), and then reacting at 90-180° C. for 1.5-6 hours, and then immersing the reaction product in water and alcohol solvent for dialysis to remove impurities, and then freeze-drying to obtain an aerogel material;
[0044] The mass ratio of the precursor material to the reducing agent is (0.2-2.5):1;
[0045] (3) Under a protective atmosphere, calcining the aerogel material in step (2) at a temperature of 900-1100° C. for 2-4 hours to obtain the silicon-oxygen composite material.
[0046] In a second aspect, the present invention provides a silicon-oxygen composite material, which is prepared by the preparation method described in the first aspect.
[0047] The silicon-oxygen composite material of the present invention comprises reduced graphene oxide coated silicon oxide material, wherein the reduced graphene oxide coats at least one silicon oxide particle; meanwhile, the silicon-oxygen composite material of the present invention is a three-dimensional porous material composed of reduced graphene oxide coated silicon oxide material.
[0048] The present invention reduces graphene oxide and coats silicon dioxide material, namely rGO@SiO x 0<x<2, for example, it can be 0.1, 0.5, 1, 1.5 or 1.8, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] In a third aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the silicon-oxygen composite material as described in the second aspect.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] (1) rGO@SiO prepared by the present invention xThe silicon-oxygen composite material has a core-shell structure of reduced graphene oxide encapsulating silicon oxide. The outer reduced graphene oxide shell can not only improve the conductivity of silicon oxide, but also inhibit the excessive volume expansion of silicon during the charge and discharge process, thereby improving the first efficiency, rate performance and cycle stability of the battery.
[0052] (2) rGO@SiO prepared by the present invention x The silicon-oxygen composite material has a three-dimensional network structure, which reserves expansion space for the internal stress caused by the expansion and contraction of silicon oxide during charging and discharging, further improving the cycle stability. The three-dimensional network structure is conducive to the transmission of lithium ions, further improving the electrochemical performance of the battery.
[0053] (3) rGO@SiO prepared by the present invention x SiO in silicon-oxygen composites x Nano-sized particles can, on the one hand, relieve the mechanical stress inside the particles and improve the stability of the particle structure; on the other hand, small-sized particles can reduce the transmission distance of lithium ions. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 This is a schematic structural diagram of a reduced graphene oxide layer covering a plurality of silicon oxide particles in the silicon-oxygen composite material described in Example 1 of the present invention;
[0055] Figure 2 This is a schematic structural diagram of a silicon oxide particle coated with a reduced graphene oxide layer in the silicon-oxygen composite material described in Example 1 of the present invention;
[0056] 1-Silicon dioxide particles, 2-Reduced graphene oxide layer. DETAILED DESCRIPTION
[0057] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0058] Example 1
[0059] This embodiment provides a method for preparing a silicon-oxygen composite material, the preparation method comprising the following steps:
[0060] (1) 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide were added to 1000 mL of graphene oxide (0.5 mg / mL) dispersion at a molar ratio of 1:1, stirred at room temperature for 30 min to activate the carboxyl group, 10 g of amino-modified silica with a particle size D50 of 100 nm was added and continued to be stirred at room temperature for 24 h, then centrifuged for solid-liquid separation, washed with water and methanol, and freeze-dried for 24 h to obtain a precursor material of graphene oxide-coated silica;
[0061] The mass ratio of the graphene oxide to the amino silicon dioxide is 0.5:10;
[0062] (2) taking 0.075 g of the precursor material described in step (1), ultrasonically dispersing it in 30 mL of deionized water to prepare a 2.5 mg / mL suspension, adding 0.03 g of ascorbic acid to the suspension, stirring and dissolving it, and then transferring it to a Teflon-lined stainless steel autoclave, reacting it at 120° C. for 3 h to obtain a hydrogel of reduced graphene oxide coated with silica, and then immersing it in deionized water and alcohol for dialysis to remove impurities, to obtain an aerogel material of reduced graphene oxide coated with silica;
[0063] The mass ratio of the precursor material to ascorbic acid is 2.5:1;
[0064] (3) In an argon atmosphere, the aerogel material of step (2) is calcined at 1000° C. for 3 h, and naturally cooled to room temperature to obtain a three-dimensional porous reduced graphene oxide-coated silicon oxide silicon-oxygen composite material, wherein the reduced graphene oxide layer 2 encapsulates a plurality of silicon oxide particles 1. Figure 1 As shown, the schematic diagram of the structure when the reduced graphene oxide layer 2 covers a silicon oxide particle 1 is as shown in Figure 2 shown.
[0065] Example 2
[0066] This embodiment provides a method for preparing a silicon-oxygen composite material, the preparation method comprising the following steps:
[0067] (1) 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide were added to 1000 mL of graphene oxide (0.5 mg / mL) dispersion at a molar ratio of 1:1, stirred at room temperature for 30 min to activate the carboxyl group, 10 g of amino-modified silica with a particle size D50 of 100 nm was added and continued to be stirred at room temperature for 24 h, then centrifuged for solid-liquid separation, washed with water and methanol, and freeze-dried for 24 h to obtain a precursor material of graphene oxide-coated silica;
[0068] The mass ratio of the graphene oxide to the amide silicon source is 0.5:10;
[0069] (2) taking 0.18 g of the precursor material described in step (1), ultrasonically dispersing it in 30 mL of deionized water to prepare a 6 mg / mL suspension, adding 0.9 g of ascorbic acid to the suspension, stirring and dissolving it, and then transferring it to a Teflon-lined stainless steel autoclave, reacting it at 120° C. for 3 h to obtain a hydrogel of reduced graphene oxide coated with silica, and then immersing it in deionized water and alcohol for dialysis to remove impurities, to obtain an aerogel material of reduced graphene oxide coated with silica;
[0070] The mass ratio of the precursor material to ascorbic acid is 0.2:1;
[0071] (3) Under an argon atmosphere, the aerogel material of step (2) is calcined at a temperature of 1000° C. for 3 h, and naturally cooled to room temperature to obtain a three-dimensional porous reduced graphene oxide-coated silicon-oxygen composite material.
[0072] Example 3
[0073] This embodiment provides a method for preparing a silicon-oxygen composite material, the preparation method comprising the following steps:
[0074] (1) 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide were added to 1000 mL of graphene oxide (0.5 mg / mL) dispersion at a molar ratio of 1:1, stirred at room temperature for 30 min to activate the carboxyl group, and amino-modified silica with a particle size D50 of 1 μm was added and stirred at room temperature for 24 h, then centrifuged for solid-liquid separation, washed with water and methanol, and freeze-dried for 24 h to obtain a precursor material of graphene oxide-coated silica;
[0075] The mass ratio of the graphene oxide to the amide silicon source is 0.5:10;
[0076] (2) taking 0.075 g of the precursor material described in step (1), ultrasonically dispersing it in 30 mL of deionized water to prepare a 2.5-6 mg / mL suspension, adding 0.04 g of sodium sulfide to the suspension, stirring and dissolving it, and then transferring it to a Teflon-lined stainless steel autoclave, reacting it at 120° C. for 3 h to obtain a hydrogel of reduced graphene oxide coated with silica, and then immersing it in deionized water and alcohol for dialysis to remove impurities, to obtain an aerogel material of reduced graphene oxide coated with silica;
[0077] The mass ratio of the precursor material to ascorbic acid is 1.875:1;
[0078] (3) Under an argon atmosphere, the aerogel material of step (2) is calcined at a temperature of 1000° C. for 3 h, and naturally cooled to room temperature to obtain a three-dimensional porous reduced graphene oxide-coated silicon-oxygen composite material.
[0079] Example 4
[0080] This embodiment provides a method for preparing a silicon-oxygen composite material, the preparation method comprising the following steps:
[0081] (1) 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide were added to 1000 mL of graphene oxide (0.1 mg / mL) dispersion at a molar ratio of 1:1, stirred at room temperature for 30 min to activate the carboxyl group, 10 g of amino-modified silica with a particle size D50 of 100 nm was added and stirred at room temperature for 24 h, then centrifuged for solid-liquid separation, washed with water and methanol, and freeze-dried for 24 h to obtain a precursor material of graphene oxide-coated silica;
[0082] The mass ratio of the graphene oxide to the amide silicon source is 0.1:10;
[0083] (2) 0.075 g of the precursor material described in step (1) was ultrasonically dispersed in 30 mL of deionized water to prepare a 4 mg / mL suspension, 0.03 g of ascorbic acid was added to the suspension, and after stirring and dissolving, it was transferred to a Teflon-lined stainless steel autoclave and reacted at 150° C. for 6 h to obtain a hydrogel of reduced graphene oxide coated with silica, which was then immersed in deionized water and alcohol for dialyzing to remove impurities to obtain an aerogel material of reduced graphene oxide coated with silica;
[0084] The mass ratio of the precursor material to ascorbic acid is 2.5:1;
[0085] (3) Under an argon atmosphere, the aerogel material of step (2) is calcined at 900° C. for 4 h, and naturally cooled to room temperature to obtain a three-dimensional porous reduced graphene oxide-coated silicon-oxygen composite material.
[0086] Example 5
[0087] This embodiment provides a method for preparing a silicon-oxygen composite material, the preparation method comprising the following steps:
[0088] (1) 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide were added to 1000 mL of graphene oxide (1 mg / mL) dispersion at a molar ratio of 1:1, stirred at room temperature for 30 min to activate the carboxyl group, and amino-modified silica with a particle size D50 of 1 μm was added and stirred at room temperature for 24 h, then centrifuged for solid-liquid separation, washed with water and methanol, and freeze-dried for 24 h to obtain a precursor material of graphene oxide-coated silica;
[0089] The mass ratio of the graphene oxide to the amide silicon source is 1:10;
[0090] (2) taking 0.075 g of the precursor material described in step (1), ultrasonically dispersing it in 30 mL of deionized water to prepare a 2.5 mg / mL suspension, adding 0.03 g of ascorbic acid to the suspension, stirring and dissolving it, and then transferring it to a Teflon-lined stainless steel autoclave, reacting it at 180° C. for 1.5 h to obtain a hydrogel of reduced graphene oxide coated with silica, and then immersing it in deionized water and alcohol for dialyzing to remove impurities, to obtain an aerogel material of reduced graphene oxide coated with silica;
[0091] The mass ratio of the precursor material to ascorbic acid is 2.5:1;
[0092] (3) Under an argon atmosphere, the aerogel material of step (2) is calcined at a temperature of 1100° C. for 2 h, and naturally cooled to room temperature to obtain a three-dimensional porous reduced graphene oxide-coated silicon-oxygen composite material.
[0093] Example 6
[0094] This embodiment provides a method for preparing a silicon-oxygen composite material. The preparation method is the same as that of Embodiment 1 except that the particle size D50 of the amino silicon dioxide in step (1) is 5 μm.
[0095] Example 7
[0096] This embodiment provides a method for preparing a silicon-oxygen composite material. The preparation method is the same as that of Embodiment 1 except that the particle size D50 of the amino silicon dioxide in step (1) is 6 μm.
[0097] Example 8
[0098] This embodiment provides a method for preparing a silicon-oxygen composite material. The preparation method is the same as that of Embodiment 1 except that the particle size D50 of the amino-silica in step (1) is 20 nm.
[0099] Example 9
[0100] This embodiment provides a method for preparing a silicon-oxygen composite material. The preparation method is the same as that of Embodiment 1 except that the mass ratio of graphene oxide to amino-treated silicon dioxide in step (1) is 0.05:10.
[0101] Example 10
[0102] This embodiment provides a method for preparing a silicon-oxygen composite material. The preparation method is the same as that of Embodiment 1 except that the mass ratio of graphene oxide to amino-treated silicon dioxide in step (1) is 1.3:10.
[0103] Embodiment 11
[0104] This embodiment provides a method for preparing a silicon-oxygen composite material. The preparation method is the same as that of Embodiment 1 except that the reaction temperature in step (2) is 80° C.
[0105] Example 12
[0106] This embodiment provides a method for preparing a silicon-oxygen composite material. The preparation method is the same as that of Embodiment 1 except that the reaction temperature in step (2) is 200° C.
[0107] Comparative Example 1
[0108] This comparative example provides a method for preparing a silicon-oxygen composite material, the preparation method comprising the following steps:
[0109] (1) 0.075 g of graphene oxide was ultrasonically dispersed in 30 mL of deionized water to prepare a 2.5 mg / mL GO suspension, 0.03 g of ascorbic acid was added, the mixture was stirred and dissolved, and the mixture was transferred to a Teflon-lined stainless steel autoclave, and reacted at 120 ° C for 3 h to obtain a reduced graphene oxide hydrogel, which was then immersed in deionized water and alcohol for dialysis to remove impurities, and freeze-dried to obtain a reduced graphene oxide aerogel;
[0110] (2) Mixing the reduced graphene oxide aerogel and silicon dioxide with a particle size D50 of 100 nm, grinding the mixture, transferring the mixture to a sintering furnace, introducing argon gas at high temperature, keeping the mixture at 1000° C. for 3 h, and naturally cooling the mixture to room temperature to obtain a silicon-oxygen composite material;
[0111] The mass ratio of the reduced graphene oxide aerogel to silicon dioxide is 0.5:10.
[0112] Comparative Example 2
[0113] This comparative example provides a method for preparing a silicon-oxygen composite material, the preparation method comprising the following steps:
[0114] (1) 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide were added to 1000 mL of graphene oxide (0.5 mg / mL) dispersion at a molar ratio of 1:1, and stirred at room temperature for 30 min to activate the carboxyl groups. Then, 10 g of amino-modified silica with a particle size of 100 nm was added to the mixed solution, and stirring was continued at room temperature for 24 h. The solid-liquid separation was performed by centrifugation, washed with water and methanol, and freeze-dried to obtain a 24-hour graphene oxide-coated silica precursor.
[0115] (2) 0.075 g GO@SiO2 was ultrasonically dispersed in 30 mL deionized water to prepare a 2.5 mg / mL GO suspension, 0.03 g ascorbic acid was added, and the mixture was reacted at 120 °C with magnetic stirring for 3 h. The mixture was centrifuged, washed, and dried to obtain rGO@SiO2 powder.
[0116] The rGO@SiO2 powder was transferred to a sintering furnace, argon was introduced at high temperature, and the temperature was kept at 1000℃ for 3h, and then naturally cooled to room temperature to obtain rGO@SiO x Composite negative electrode materials.
[0117] The silicon-oxygen composite materials obtained in the above examples and comparative examples were prepared into negative electrode sheets, and batteries were formed with NCM811 positive electrode sheets, polyethylene separators and lithium hexafluorophosphate electrolytes. The electrochemical performance of the batteries was tested under 0.1C and 0.5C charge and discharge conditions. The test results are shown in Table 1:
[0118] Table 1
[0119]
[0120]
[0121] From Table 1 we can see that:
[0122] The silicon-oxygen composite material obtained by the present invention has excellent electrochemical performance. It can be seen from Example 1 and Comparative Example 1 that the carboxyl groups on the surface of the graphene oxide of the present invention condense with the aminoamide on the surface of the amino silicon source to generate a precursor with strong binding ability, thereby improving the electrochemical performance of the material. It can be seen from Example 1 and Comparative Example 2 that the present invention first prepares a graphene oxide-coated silica precursor and then performs a hydrothermal reaction in step (2) to obtain a material with better performance. If step (1) and step (2) are combined and performed, agglomeration occurs between the silica particles, and the graphene oxide preferentially interacts with each other to form a three-dimensional structure after being reduced, and a three-dimensional reduced graphene oxide-coated silica structure cannot be formed. It can be seen from Example 1 and Examples 6-13 that the particle size of the amino silicon dioxide of the present invention, the coating amount of the coating layer, the hydrothermal reaction in step (2) and the temperature of the hydrothermal reaction in step (2) will affect the material performance, thereby affecting the battery performance.
[0123] In summary, the present invention provides a silicon-oxygen composite material and a preparation method and application thereof. The preparation method can obtain a silicon-oxygen gel material coated with reduced graphene oxide through redox self-assembly, and finally obtain a three-dimensional porous silicon-oxygen composite material through calcination, which reserves space for the expansion of the silicon-oxygen material and improves the conductivity of the material, thereby improving the first efficiency, rate performance and cycle stability of the battery.
[0124] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a silicon-oxygen composite material, It is characterized in that The preparation method comprises the following steps: (1) mixing carboxylated graphene oxide, an amino silicon source and a solvent, performing solid-liquid separation and drying to obtain a precursor material; (2) mixing and reacting the precursor material, reducing agent and solvent described in step (1), and then drying to obtain an aerogel material; (3) calcining the aerogel material of step (2) to obtain the silicon-oxygen composite material.
2. The preparation method according to claim 1, It is characterized in that The particle size D50 of the amide silicon source in step (1) is 0.1-5 μm; Preferably, the amide silicon source in step (1) comprises amide silicon dioxide; Preferably, the mass ratio of the carboxylated graphene oxide to the amino silicon source in step (1) is (0.1-1):
10.
3. The preparation method according to claim 1 or 2, It is characterized in that The method for preparing the carboxylated graphene oxide in step (1) comprises: mixing a dispersion of carbodiimide hydrochloride, an imide compound and graphene oxide; Preferably, the carbodiimide hydrochloride comprises 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride; Preferably, the imide compound comprises N-hydroxysuccinimide; Preferably, washing is performed between the solid-liquid separation and drying in step (1); Preferably, the drying method in step (1) includes freeze-drying.
4. The preparation method according to any one of claims 1 to 3, It is characterized in that The reaction temperature in step (2) is 90-180°C, preferably 120-180°C; Preferably, the reaction time in step (2) is 1.5-6h; Preferably, the reaction in step (2) is a hydrothermal reaction carried out in a reactor; Preferably, in the mixed solution obtained by mixing in step (2), the concentration of the precursor material is 2.5-6 mg / mL.
5. The preparation method according to any one of claims 1 to 4, It is characterized in that The drying method in step (2) includes freeze drying; Preferably, after the reaction in step (2), impurities are first removed and then dried; Preferably, the impurity removal method includes immersing in water and alcohol solvents for dialysis removal.
6. The preparation method according to any one of claims 1 to 5, It is characterized in that The mass ratio of the precursor material and the reducing agent in step (2) is (0.2-2.5):1; Preferably, the reducing agent in step (2) comprises any one of sodium bisulphite formaldehyde, sodium sulfide, ascorbic acid, hydrogen iodide or hydroquinone, or a combination of at least two thereof.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that The calcination temperature in step (3) is 900-1100° C. and the calcination time is 2-4 hours; Preferably, the calcination in step (3) is carried out under a protective atmosphere.
8. The preparation method according to any one of claims 1 to 7, It is characterized in that The preparation method comprises the following steps: (1) mixing a dispersion of carbodiimide hydrochloride, an imide compound and graphene oxide, then adding an amide silicon source to the mixed solution and continuing to mix, and then performing solid-liquid separation, washing and freeze-drying to obtain a precursor material; The amino silicon source is amino silicon dioxide with a particle size D50 of 0.1-5 μm; (2) mixing the precursor material, reducing agent and solvent described in step (1), and then reacting at 90-180° C. for 1.5-6 hours, and then immersing the reaction product in water and alcohol solvent for dialysis to remove impurities, and then freeze-drying to obtain an aerogel material; The mass ratio of the precursor material to the reducing agent is (0.2-2.5):1; (3) Under a protective atmosphere, calcining the aerogel material in step (2) at a temperature of 900-1100° C. for 2-4 hours to obtain the silicon-oxygen composite material.
9. A silicon-oxygen composite material, It is characterized in that The silicon-oxygen composite material is prepared by the preparation method according to any one of claims 1 to 8.
10. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the silicon-oxygen composite material as claimed in claim 9.
Citation Information
Patent Citations
Core-shell graphene-silicon composite material, preparation method thereof, electrode material and battery
CN110112380A
Preparation method of negative electrode material, negative electrode material and application
CN113555536A
Nano silicon dioxide / graphene high-density composite silicon-carbon negative electrode material and preparation method and application thereof
CN115548319A
Graphene chemically bonded carbon-coated silicon composite material and preparation method and application thereof
CN117334876A
Conducting polymer network-protected cathode active materials for lithium secondary batteries
US20210296650A1
Cited By
Composite particles, method for producing the composite particles, gas separation membrane, method for producing the gas separation membrane, gas separation module, and gas separation apparatus
JP7712013B1
Composite particles, method for manufacturing composite particles, gas separation membrane, method for manufacturing a gas separation membrane, gas separation module and gas separation device
KR1020260085267A
Composite particles, method for manufacturing composite particles, gas separation membrane, method for manufacturing a gas separation membrane, gas separation module and gas separation device
KR102995651B1
Composite particles, method for producing composite particles, gas separation membrane, method for producing gas separation membrane, gas separation module, and gas separation device
WO2026115763A1