Preparation method of adsorbent precipitated silica

By using the reaction of low-heavy metal solid sodium silicate and sulfuric acid solution and surfactant treatment in the preparation of silica, the existing problems of small particle size and low pore volume of silica are solved, and high adsorption and fluidity are prepared. Silica particles are suitable for effective adsorption and stable storage of vitamins in feed.

CN118851187APending Publication Date: 2024-10-29ANHUI QUECHEN SILICON CHEM CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410906358.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing silica has small particle size and low pore volume, resulting in poor adsorption performance and affecting its application in feed.

Method used

Use low-heavy metal solid sodium silicate with a modulus of 2.5 to 3.0 to react with a 30 to 50 wt% sulfuric acid solution, add the surfactant sorbitol laurate, control the reaction pH and temperature, and prepare a product with the properties of Silica particles with high specific surface area and high oil absorption value.

Benefits of technology

The prepared silica has good adsorption and fluidity, can effectively absorb vitamins and maintain long-term stability, and is not easy to desorb.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of adsorbent precipitated silica, and relates to the technical field of silica, the preparation method comprises the following steps: S1, selecting low heavy metal solid sodium silicate with the modulus of 2.5-3.0 to prepare a sodium silicate solution with the concentration of 15-20wt%; preparing a certain volume of sulfuric acid solution with the concentration of 30-50wt%; s2, adding industrial water into the reaction kettle as a reaction base solution; s3, adding the prepared sodium silicate solution into a reaction kettle, adding the prepared sulfuric acid solution in a stirring state, and reacting; and S4, continuously adding the prepared sulfuric acid and sodium silicate solution into the reaction kettle, adding a surfactant, and keeping the pH value of the reaction system at 7.5-9.5. According to the invention, sorbitol laurate is adopted as a surfactant, so that silicon dioxide has a loose and porous structure, the pore size is increased, and the prepared silicon dioxide has the characteristics of low specific surface area, high oil absorption value, good adsorbability and good fluidity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon dioxide, in particular to a method for preparing adsorbent precipitated silicon dioxide. Background Art

[0002] Precipitated hydrated silica, also known as white carbon black, belongs to the field of inorganic silicates. It is an excellent porous material that is non-toxic, harmless, pollution-free, and has no toxic side effects. It is an important inorganic chemical raw material and can be used as a carrier or flow agent in the pesticide, feed and other industries.

[0003] Feed additives play an irreplaceable role in feed. They can balance the nutritional components of feed, strengthen the nutritional value of basic feed, improve animal production performance, ensure animal health, and increase feed utilization. Silicon dioxide can be used as a flow aid and anti-caking agent for various premixes and trace mineral raw materials in feed and feed additives, and can also be used as a carrier. When the adsorption amount is large, the powder can still maintain good fluidity.

[0004] The disadvantages of the prior art are that the silica particles in the prior art have a small particle size and a low pore volume, resulting in poor adsorption performance of the silica particles, and less active ingredients can be carried in the preparation of feed, thus affecting its application. Therefore, those skilled in the art provide a method for preparing adsorbent precipitated silica to solve the problems raised in the above background technology. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing adsorbent precipitated silica to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing adsorbent precipitated silica, which specifically comprises the following steps:

[0007] S1: Select low-heavy metal solid sodium silicate with a modulus of 2.5 to 3.0 to prepare a sodium silicate solution with a concentration of 15 to 20 wt%; prepare a certain volume of sulfuric acid solution with a concentration of 30 to 50 wt%;

[0008] S2: Add industrial water as reaction base liquid into the reactor and heat it to 30-40°C;

[0009] S3: Add the prepared sodium silicate solution into the reactor, heat the solution to 55-75°C, set the stirring speed to 300-500r / min, add the prepared sulfuric acid solution under stirring, adjust the pH value of the reaction system to 7.5-9.5, stop when the reaction liquid reaches 2 / 3 of the volume of the reactor, and control the feeding time within 30min;

[0010] S4: Continue to add the prepared sulfuric acid and sodium silicate solution to the reactor, and add a surfactant, keep the pH value of the reaction system within 7.5 to 9.5, and the reaction temperature within 55 to 75°C. After reacting for 40 to 60 minutes, stop adding the sodium silicate solution, and continue to add sulfuric acid solution until the pH value of the reaction system is 3.5 to 5.5, and the reaction is completed, and the reaction is aged for 1.0 to 1.5 hours;

[0011] S5: The reaction liquid is filtered and washed with industrial water, and then directly sent to a pulping machine to form a thick pulp;

[0012] S6: sending the concentrated slurry into a spray dryer for drying to obtain granular silicon dioxide;

[0013] Wherein, the surfactant is sorbitan laurate.

[0014] As a further solution of the present invention: the mass ratio of the surfactant to the silicon dioxide in the water glass is 0.2-10.5%.

[0015] As a further solution of the present invention: the amount of industrial water added to S2 is 1 / 6 of the volume of the reactor.

[0016] As a further solution of the present invention: in S5, the content of sodium sulfate in the filter cake is determined by the conductivity of the washing water, and the sodium sulfate content of the final product is controlled to be less than 2%, and the solid content of the filter cake is controlled to be 20-25%.

[0017] As a further solution of the present invention: the BET of the silicon dioxide is 135 to 175 m 2 / g.

[0018] As a further solution of the present invention: the oil absorption value of the silica is 250-300 mL / 100 g.

[0019] As a further solution of the present invention: the bulk density of the silicon dioxide is 250-350 g / L.

[0020] As a further solution of the present invention: the median diameter (D50) of the silica is 200 to 300 um.

[0021] As a further solution of the present invention: the heating loss of the silicon dioxide is ≤6.0%.

[0022] As a further solution of the present invention: the loss on ignition of silicon dioxide is ≤6.0%.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The silicon dioxide prepared by the preparation method of the present invention has the characteristics of low specific surface area, high oil absorption value, good adsorption and fluidity, and its BET is 135-175m2 / g, oil absorption value is 250~300mL / 100g, and median diameter (D50) is 200~300um.

[0025] 2. The preparation method of the present invention uses sorbitol laurate as a surfactant, so that the silicon dioxide obtains a loose and porous structure and increases the pore size. When the silicon dioxide particles are mixed with vitamins, they can absorb a large amount of vitamins and have long-term storage stability and are not easy to desorb. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] In the embodiment of the present invention,

[0028] Example 1

[0029] A method for preparing adsorbent precipitated silica, comprising the following steps:

[0030] S1: Select low-heavy metal solid sodium silicate with a modulus of 2.5 to prepare a sodium silicate solution with a concentration of 15wt%; prepare a certain volume of sulfuric acid solution with a concentration of 30wt%;

[0031] S2: Add industrial water as the reaction base liquid into the reactor, the amount of industrial water added is 1 / 6 of the volume of the reactor, and heat it to 30°C;

[0032] S3: Add the prepared sodium silicate solution into the reactor, heat the solution to 55°C, set the stirring speed to 300r / min, add the prepared sulfuric acid solution under stirring, adjust the pH value of the reaction system to 7.5, and stop when the reaction liquid reaches 2 / 3 of the volume of the reactor. The feeding time is controlled within 30min;

[0033] S4: Continue to add the prepared sulfuric acid and sodium silicate solution to the reactor, and add the surfactant sorbitol laurate, maintain the pH value of the reaction system at 7.5, the reaction temperature at 55°C, stop adding the sodium silicate solution after reacting for 40 minutes, continue to add the sulfuric acid solution until the reaction ends when the pH value of the reaction system reaches 3.5, and age for 1.0 hour;

[0034] S5: The reaction liquid is filtered and washed with industrial water, and then directly sent to a pulping machine to form a thick slurry. The sodium sulfate content in the filter cake is determined by the conductivity of the washing water. The sodium sulfate content of the final product is controlled to be less than 2%, and the solid content of the filter cake is controlled to be 20%;

[0035] S6: The concentrated slurry is sent to a spray dryer for drying, using hot air from natural gas combustion as a heat source to obtain granular silicon dioxide.

[0036] The mass ratio of the surfactant to the silicon dioxide in the water glass is 0.2%.

[0037] Example 2

[0038] A method for preparing adsorbent precipitated silica, comprising the following steps:

[0039] S1: Select low-heavy metal solid sodium silicate with a modulus of 3.0 to prepare a sodium silicate solution with a concentration of 20wt%; prepare a certain volume of sulfuric acid solution with a concentration of 50wt%;

[0040] S2: Add industrial water as the reaction base liquid into the reactor, the amount of industrial water added is 1 / 6 of the volume of the reactor, and heat it to 40°C;

[0041] S3: Add the prepared sodium silicate solution into the reactor, heat the solution to 75°C, set the stirring speed to 500r / min, add the prepared sulfuric acid solution under stirring, adjust the pH value of the reaction system to 9.5, and stop when the reaction liquid reaches 2 / 3 of the volume of the reactor. The feeding time is controlled within 30min;

[0042] S4: Continue to add the prepared sulfuric acid and sodium silicate solution into the reactor, and add the surfactant sorbitol laurate, keep the pH value of the reaction system at 9.5, the reaction temperature at 75°C, stop adding the sodium silicate solution after reacting for 60 minutes, continue to add the sulfuric acid solution until the reaction ends when the pH value of the reaction system reaches 5.5, and age for 1.5 hours;

[0043] S5: The reaction liquid is filtered and washed with industrial water, and then directly sent to a pulping machine to form a thick slurry. The sodium sulfate content in the filter cake is determined by the conductivity of the washing water. The sodium sulfate content of the final product is controlled to be less than 2%, and the solid content of the filter cake is controlled to be 25%;

[0044] S6: The concentrated slurry is sent to a spray dryer for drying, using hot air from natural gas combustion as a heat source to obtain granular silicon dioxide.

[0045] The mass ratio of the surfactant to the silicon dioxide in the water glass is 10.5%.

[0046] Example 3

[0047] A method for preparing adsorbent precipitated silica, comprising the following steps:

[0048] S1: Select low-heavy metal solid sodium silicate with a modulus of 2.7 to prepare a sodium silicate solution with a concentration of 18wt%; prepare a certain volume of sulfuric acid solution with a concentration of 40wt%;

[0049] S2: Add industrial water as the reaction base liquid into the reactor, the amount of industrial water added is 1 / 6 of the volume of the reactor, and heat it to 35°C;

[0050] S3: Add the prepared sodium silicate solution into the reactor, heat the solution to 65°C, set the stirring speed to 400r / min, add the prepared sulfuric acid solution under stirring, adjust the pH value of the reaction system to 8.5, and stop when the reaction liquid reaches 2 / 3 of the volume of the reactor. The feeding time is controlled within 30min;

[0051] S4: Continue to add the prepared sulfuric acid and sodium silicate solution to the reactor, and add the surfactant sorbitol laurate, keep the pH value of the reaction system at 8.5, the reaction temperature at 65°C, stop adding the sodium silicate solution after reacting for 50 minutes, continue to add the sulfuric acid solution until the reaction ends when the pH value of the reaction system reaches 4.5, and age for 1.2 hours;

[0052] S5: The reaction liquid is filtered and washed with industrial water, and then directly sent to a pulping machine to form a thick slurry. The sodium sulfate content in the filter cake is determined by the conductivity of the washing water. The sodium sulfate content of the final product is controlled to be less than 2%, and the solid content of the filter cake is controlled to be 22%;

[0053] S6: The concentrated slurry is sent to a spray dryer for drying, using hot air from natural gas combustion as a heat source to obtain granular silicon dioxide.

[0054] The mass ratio of the surfactant to the silicon dioxide in the water glass is 5%.

[0055] The performance of the silicon dioxide products obtained in Examples 1 to 3 was tested. The BET of the silicon dioxide of the present invention was 135 to 175 m 2 / g, bulk density is 250-350g / L, oil absorption value is 250-300mL / 100g, median diameter (D50) is 200-300um, pH (5% aqueous solution) is 6.0-7.5, silicon dioxide content (ignition product) is ≥97%, heating loss is ≤6.0%, ignition loss is ≤6.0%, heavy metal (in terms of Pb) is ≤0.003%, arsenic content is ≤0.0003%, lead content is ≤0.001%, and soluble salt is ≤2.0%.

[0056] In summary, the silica prepared by the preparation method of the present invention has the characteristics of low specific surface area, high oil absorption value, good adsorption and fluidity. The preparation method of the present invention adopts sorbitol laurate as a surfactant, so that the silica obtains a loose and porous structure, and increases the pore size. When the silica particles are mixed with vitamins, they can absorb a large amount of vitamins, and can maintain long-term storage stability and is not easy to desorb.

[0057] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0058] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing adsorbent precipitated silica, characterized in that: The specific steps include: S1: Select low-heavy metal solid sodium silicate with a modulus of 2.5 to 3.0 to prepare a sodium silicate solution with a concentration of 15 to 20 wt%; prepare a certain volume of sulfuric acid solution with a concentration of 30 to 50 wt%; S2: Add industrial water as reaction base liquid into the reactor and heat it to 30-40°C; S3: Add the prepared sodium silicate solution into the reactor, heat the solution to 55-75°C, set the stirring speed to 300-500r / min, add the prepared sulfuric acid solution under stirring, adjust the pH value of the reaction system to 7.5-9.5, stop when the reaction liquid reaches 2 / 3 of the volume of the reactor, and control the feeding time within 30min; S4: Continue to add the prepared sulfuric acid and sodium silicate solution to the reactor, and add a surfactant, keep the pH value of the reaction system within 7.5 to 9.5, and the reaction temperature within 55 to 75°C. After reacting for 40 to 60 minutes, stop adding the sodium silicate solution, and continue to add sulfuric acid solution until the pH value of the reaction system is 3.5 to 5.5, and the reaction is completed, and the reaction is aged for 1.0 to 1.5 hours; S5: The reaction liquid is filtered and washed with industrial water, and then directly sent to a pulping machine to form a thick pulp; S6: sending the concentrated slurry into a spray dryer for drying to obtain granular silicon dioxide; Wherein, the surfactant is sorbitan laurate.

2. The method for preparing adsorbent precipitated silica according to claim 1, characterized in that: The mass ratio of the surfactant to the silicon dioxide in the water glass is 0.2-10.5%.

3. The method for preparing adsorbent precipitated silica according to claim 1, characterized in that: The amount of industrial water added to S2 is 1 / 6 of the volume of the reactor.

4. The method for preparing adsorbent precipitated silica according to claim 1, characterized in that: In S5, the content of sodium sulfate in the filter cake is determined by the conductivity of the washing water, and the sodium sulfate content of the final product is controlled to be less than 2%, and the solid content of the filter cake is controlled to be 20-25%.

5. The method for preparing adsorbent precipitated silica according to claim 1, characterized in that: The silicon dioxide BET is 135 to 175 m 2 / g.

6. The method for preparing adsorbent precipitated silica according to claim 1, characterized in that: The silica oil absorption value is 250-300 mL / 100 g.

7. The method for preparing adsorbent precipitated silica according to claim 1, characterized in that: The bulk density of the silicon dioxide is 250-350 g / L.

8. The method for preparing adsorbent precipitated silica according to claim 1, characterized in that: The median diameter (D50) of the silicon dioxide is 200 to 300 um.

9. The method for preparing adsorbent precipitated silica according to claim 1, characterized in that: The silicon dioxide loses weight by heating ≤ 6.0%.

10. The method for preparing adsorbent precipitated silica according to claim 1, characterized in that: The silicon dioxide has a loss on ignition of ≤6.0%.

Citation Information

Patent Citations

  • Large-pore-volume high-adsorption silicon dioxide additive and preparation method thereof

    CN112194147A

  • Washing machine

    KR1020250136684A

  • High-specific-surface-area high-VOC-adsorption silicon dioxide and preparation method therefor

    WO2020098273A1