Preparation method of antifouling hydrophobic photovoltaic glass

Through pretreatment and multi-layer film technology, the problem of photovoltaic glass surface being susceptible to contamination is solved, its anti-fouling, hydrophobic and conductive properties are significantly improved, and the energy conversion efficiency of solar panels is improved.

CN118851590APending Publication Date: 2024-10-29JIANGSU SIMBA NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411225602.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The surface of traditional photovoltaic glass lacks self-cleaning ability and is easily affected by pollutants, resulting in reduced light transmittance and insufficient electrical conductivity, affecting the energy conversion efficiency of solar panels.

Method used

Pretreatment, multi-layer coating technology of composite alumina sol and modified silica sol is used to form a porous composite alumina film layer and a fluorinated modified silica film layer through ultrasonic cleaning, spin coating and muffle furnace treatment. Enhance the anti-fouling, hydrophobic and conductive properties of photovoltaic glass.

Benefits of technology

It significantly improves the anti-fouling and hydrophobic ability, electrical conductivity and light transmittance of photovoltaic glass, ensuring the adhesion and performance stability of the photovoltaic glass surface.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of antifouling hydrophobic photovoltaic glass, and relates to the technical field of photovoltaics. When the antifouling hydrophobic photovoltaic glass is prepared, the photovoltaic glass is subjected to surface cleaning and surface hydroxylation to obtain pretreated photovoltaic glass, then the surface of the pretreated photovoltaic glass is coated with composite aluminum oxide sol, the pretreated photovoltaic glass is put into a muffle furnace to be subjected to second-stage heating, and primary film-coated photovoltaic glass is obtained; and then continuously coating the surface of the photovoltaic glass with the porous composite aluminum oxide film attached on the surface with the modified silicon oxide sol, drying for a period of time, and then carrying out low-temperature annealing to obtain the antifouling hydrophobic photovoltaic glass. The antifouling and hydrophobic photovoltaic glass prepared by the invention is relatively strong in antifouling and hydrophobic capacity, relatively good in conductivity, and relatively good in surface adhesiveness and light transmittance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photovoltaics, and in particular to a method for preparing anti-fouling and hydrophobic photovoltaic glass. Background Art

[0002] As a key component of solar panels, the surface characteristics of photovoltaic glass directly affect the performance and life of solar panels. The surface of traditional photovoltaic glass usually does not have the ability to self-clean and is easily affected by pollutants such as dust, rain marks, and bird droppings. These pollutants not only reduce the light transmittance of the glass, but also hinder the effective generation and collection of photogenerated carriers, thereby affecting the energy conversion efficiency of solar panels. In addition, the insufficient conductivity of photovoltaic glass also limits the efficient collection and transmission of current, resulting in energy loss and reduced system efficiency.

[0003] Therefore, the applicant prepared an anti-fouling and hydrophobic photovoltaic glass to solve the above problems. Summary of the invention

[0004] In order to solve the existing technical problems, the present invention discloses a method for preparing anti-fouling and hydrophobic photovoltaic glass, comprising the following preparation steps: (1) Pretreatment: Place the photovoltaic glass in a 20-30% detergent solution with a concentration of 50-100 times its mass and ultrasonically clean it for 30 minutes. After taking it out, rinse it with tap water until there are no bubbles. Then rinse it with deionized water until the conductivity of the rinsed water is close to that of deionized water. Then immerse the rinsed photovoltaic glass in a mixed solution of concentrated sulfuric acid and hydrogen peroxide and ultrasonically oscillate it at room temperature for 1-3 hours. After taking it out, rinse it repeatedly with deionized water and blow it dry with nitrogen for later use to obtain the pretreated photovoltaic glass. (2) Primary coating: The composite alumina sol is applied to the pre-treated photovoltaic glass by spin coating, placed in a muffle furnace for two-stage heating treatment, and then subjected to hydrothermal treatment, followed by rinsing and drying to obtain a photovoltaic glass with a primary coating; (3) Secondary coating: Spin-coat the surface of the photovoltaic glass with the primary coating with modified silica sol, dry it for a period of time, and then anneal it at low temperature to obtain anti-fouling and hydrophobic photovoltaic glass.

[0005] Furthermore, in the mixed solution of concentrated sulfuric acid and hydrogen peroxide, the volume mixing ratio of concentrated sulfuric acid to 60% hydrogen peroxide is 4:9.

[0006] Furthermore, the preparation method of the composite alumina sol is as follows: under the stirring condition of 600~800r / min, aluminum trichloride is added to ethanol, wherein the mass ratio of ethanol to aluminum trichloride is 8.2~8.4:1, and then an ethylene glycol solution of polyvinyl pyrrolidone is added, and stirring and dissolving is continued, wherein the mass of polyvinyl pyrrolidone is 0.13~0.15 times the mass of aluminum trichloride, and then 0.1mol / L silver nitrate solution is added, wherein the mass of silver nitrate is 0.065~0.075 times the mass of aluminum trichloride, and stirring and mixing is continued for 20 minutes to obtain a composite alumina sol.

[0007] Furthermore, the specific steps of the second stage heating are: heating to 140-180°C and keeping warm for 3-4 hours, then continuing to heat to 400-450°C and keeping warm for 60-90 minutes. After the second stage heating, while forming a composite alumina film layer, the film-forming aid in the composite alumina sol is ablated to form a composite alumina film layer with a porous structure.

[0008] Furthermore, the hydrothermal treatment temperature is 400-450° C., and the treatment time is 15-25 min.

[0009] Furthermore, the preparation method of the modified silica sol is as follows: In a constant temperature water bath at 60°C and magnetic stirring, L-lysine is dissolved in a mixed solution of isopropanol and deionized water, and then tetraethyl orthosilicate is added at a rate of 10-20 drops / min, the reaction is stirred for 2-3 hours, and then allowed to stand for 10 hours, wherein the molar ratio of tetraethyl orthosilicate, L-lysine, isopropanol, and deionized water is 1:0.01-0.03:2.5:150-300; subsequently, a fluorinated silane coupling agent and ethanol are added, and stirring is continued at 60°C for 2 hours to obtain a modified silica sol, wherein the molar ratio of tetraethyl orthosilicate, fluorinated silane coupling agent, and ethanol is 1:1-3:5-8.

[0010] Furthermore, the fluorine-containing silane coupling agent includes any one or more combinations of 1H,1H,2H,2H-perfluorodecyltriethoxysilane, 1H,1H,2H,2H-perfluorooctyltriethoxysilane, 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, dodecafluoroheptylpropylmethyldimethoxysilane, dodecafluoroheptylpropyltrimethoxysilane, 3,3,3-trifluoropropylmethyldimethoxysilane, and 3.3,3-trifluoropropyltrimethoxysilane.

[0011] Furthermore, the drying temperature is 80° C. and the drying time is 30 minutes.

[0012] Furthermore, the low-temperature annealing temperature is 200° C. and the time is 2 hours.

[0013] Furthermore, the coating thickness of the composite alumina sol and the modified silica sol is 150-250 μm.

[0014] Compared with the prior art, the present invention has the following beneficial effects: When preparing the anti-fouling and hydrophobic photovoltaic glass according to the present invention, the surface of the photovoltaic glass is first cleaned and hydroxylated to obtain a pretreated photovoltaic glass, and then a composite alumina sol is coated on the surface of the pretreated photovoltaic glass and the glass is placed in a muffle furnace for two-stage heating to obtain a once-coated photovoltaic glass; then, the surface of the photovoltaic glass with a porous composite alumina film attached to the surface is further coated with a modified silica sol, and after drying for a period of time, low-temperature annealing is performed to obtain the anti-fouling and hydrophobic photovoltaic glass. The prepared anti-fouling and hydrophobic photovoltaic glass has strong anti-fouling and hydrophobic ability, good electrical conductivity, and good surface adhesion and light transmittance.

[0015] The present invention first cleans and hydroxylates the surface of the photovoltaic glass to obtain the pretreated photovoltaic glass, which can increase the hydrophilicity of the photovoltaic glass surface and increase the bonding force between the film formed by the composite alumina sol and the photovoltaic glass.

[0016] The present invention adopts aluminum chloride as a raw material to prepare an alumina sol, and adds an ethylene glycol solution of polyvinyl pyrrolidone and a silver nitrate solution to prepare a composite alumina sol. The composite alumina sol is subsequently coated on a pretreated photovoltaic glass surface and then subjected to a second-stage temperature increase to form a porous silver nanowire composite alumina film layer on the photovoltaic glass surface. The aluminum chloride reacts with alcohol to form a large amount of free chloride ions in the alumina sol, and the silver nitrate, chloride ions and polyvinyl pyrrolidone act synergistically to uniformly grow silver nanowires in the alumina sol, thereby changing the roughness of the composite alumina film layer, thereby enhancing the bonding force between the fluorinated modified silicon oxide film layer and the alumina film layer, preventing the fluorinated modified silicon oxide film layer from peeling off, and at the same time forming a conductive network on the photovoltaic glass surface, thereby enhancing the conductive performance of the photovoltaic glass. Compared with the conventional direct addition of silver nanowires, the above technical solution can avoid a large amount of agglomeration of silver nanowires, thereby ensuring the light transmittance of the anti-fouling and hydrophobic photovoltaic glass and the adhesion performance of the thin film on the surface of the photovoltaic glass.

[0017] The present invention uses fluorinated siloxane-modified silica sol to perform secondary coating on the surface of photovoltaic glass that has been coated once. Surface fluorination of nano-silica can reduce the surface energy of nano-silica, thereby enhancing the anti-fouling and hydrophobic performance of the anti-fouling and hydrophobic photovoltaic glass. The formed surface fluorinated nano-silica is filled in the pores of the composite alumina film layer with a porous structure to form a micro-nano structure, thereby further enhancing the anti-fouling and hydrophobic performance of the anti-fouling and hydrophobic photovoltaic glass. DETAILED DESCRIPTION

[0018] The present invention is further described in detail below in conjunction with examples, but the following examples should not be construed as limiting the present invention.

[0019] Some of the raw materials of the embodiments of the present invention and the comparative examples are as follows: The polyvinyl pyrrolidone was obtained from Shanghai MacLean Biochemical Technology Co., Ltd., with a molecular weight of 130,000; The fluorinated silane coupling agent is commercially available 1H,1H,2H,2H-perfluorodecyltriethoxysilane; The silver nanowires were obtained from Jiangsu Xianfeng Nanomaterials Technology Co., Ltd. and had a diameter of 30 nm and a length of 20 μm. Example

[0020] A method for preparing antifouling hydrophobic photovoltaic glass, the preparation steps are as follows: (1) Pretreatment: Place the photovoltaic glass in a 20% detergent solution with a volume 50 times its mass and perform ultrasonic cleaning for 30 minutes. After taking it out, rinse it with tap water until there are no bubbles. Rinse it with deionized water until the conductivity of the rinsed water is close to that of deionized water. Then immerse the rinsed photovoltaic glass in a mixed solution of concentrated sulfuric acid and hydrogen peroxide and perform ultrasonic oscillation at room temperature for 1 hour. After taking it out, rinse it repeatedly with deionized water and blow it dry with nitrogen for later use to obtain the pretreated photovoltaic glass. The volume ratio of concentrated sulfuric acid to 60% hydrogen peroxide in the mixed solution of concentrated sulfuric acid and hydrogen peroxide is 4:9. (2) Primary coating: Spin coating the composite alumina sol onto the pretreated photovoltaic glass. The thickness of the spin coating liquid is adjusted to 150 μm by controlling the rotation speed and time of the turntable. After coating, the glass is placed in a muffle furnace and heated to 140°C and kept at this temperature for 3 h. The temperature is then raised to 400°C and kept at this temperature for 60 min. The furnace is allowed to cool naturally to room temperature, and the glass is taken out and then placed in deionized water at 80°C for hydrothermal treatment for 15 min. After the treatment, the glass is rinsed with deionized water and dried with nitrogen to obtain a photovoltaic glass with a primary coating. (3) Secondary coating: Spin-coat 150 μm modified nano-silica sol on the surface of the primary coated photovoltaic glass, then dry it in an electric oven at 80 °C for 30 min, and then anneal it in a muffle furnace for 2 h at a low temperature of 200 °C to obtain anti-fouling and hydrophobic photovoltaic glass; The preparation method of the composite alumina sol is as follows: under a stirring condition of 600 r / min, aluminum chloride is added to ethanol, wherein the mass ratio of ethanol to aluminum chloride is 8.2:1, then an ethylene glycol solution of polyvinyl pyrrolidone is added, and stirring and dissolving is continued, wherein the mass of polyvinyl pyrrolidone is 0.13 times the mass of aluminum chloride, and then a 0.1 mol / L silver nitrate solution is added, wherein the mass of silver nitrate is 0.065 times the mass of aluminum chloride, and stirring and mixing is continued for 20 minutes to obtain a composite alumina sol.

[0021] The preparation method of the modified silica sol is as follows: in a constant temperature water bath at 60° C. and under magnetic stirring, L-lysine is dissolved in a mixed solution of isopropanol and deionized water, and then tetraethyl orthosilicate is added at a rate of 10 drops / min, stirred for reaction for 2 hours, and then allowed to stand for 10 hours, wherein the molar ratio of tetraethyl orthosilicate, L-lysine, isopropanol, and deionized water is 1:0.01:2.5:150; subsequently, a fluorinated silane coupling agent and ethanol are added, and stirring is continued at 60° C. for 2 hours to obtain a modified silica sol, wherein the molar ratio of tetraethyl orthosilicate, the fluorinated silane coupling agent, and ethanol is 1:1:5. Example

[0022] A method for preparing antifouling hydrophobic photovoltaic glass, the preparation steps are as follows: (1) Pretreatment: Place the photovoltaic glass in a 25% detergent solution with a volume of 80 times its mass and perform ultrasonic cleaning for 30 minutes. After taking it out, rinse it with tap water until there are no bubbles. Rinse it with deionized water until the conductivity of the rinsed water is close to that of deionized water. Then immerse the rinsed photovoltaic glass in a mixed solution of concentrated sulfuric acid and hydrogen peroxide and perform ultrasonic oscillation at room temperature for 2 hours. After taking it out, rinse it repeatedly with deionized water and blow it dry with nitrogen for later use to obtain the pretreated photovoltaic glass. The volume ratio of concentrated sulfuric acid to 60% hydrogen peroxide in the mixed solution of concentrated sulfuric acid and hydrogen peroxide is 4:9. (2) Primary coating: Spin coating the composite alumina sol onto the pretreated photovoltaic glass. The thickness of the spin coating liquid is adjusted to 200 μm by controlling the rotation speed and time of the turntable. After coating, the glass is placed in a muffle furnace and heated to 160°C and kept warm for 3.5 hours. The temperature is then raised to 430°C and kept warm for 75 minutes. The furnace is allowed to cool naturally to room temperature, taken out, and then placed in deionized water at 88°C for hydrothermal treatment for 20 minutes. After the treatment, the glass is rinsed with deionized water and dried with nitrogen to obtain a photovoltaic glass with a primary coating. (3) Secondary coating: Spin-coat 200 μm modified nano-silica sol on the surface of the primary coated photovoltaic glass, then dry it in an electric oven at 80 °C for 30 min, and then anneal it in a muffle furnace for 2 h at a low temperature of 200 °C to obtain anti-fouling and hydrophobic photovoltaic glass; The preparation method of the composite alumina sol is as follows: under a stirring condition of 700 r / min, aluminum chloride is added to ethanol, wherein the mass ratio of ethanol to aluminum chloride is 8.3:1, then an ethylene glycol solution of polyvinyl pyrrolidone is added, and stirring and dissolving is continued, wherein the mass of polyvinyl pyrrolidone is 0.14 times the mass of aluminum chloride, and then a 0.1 mol / L silver nitrate solution is added, wherein the mass of silver nitrate is 0.07 times the mass of aluminum chloride, and stirring and mixing is continued for 20 minutes to obtain a composite alumina sol.

[0023] The preparation method of the modified silica sol is as follows: in a constant temperature water bath at 60° C. and under magnetic stirring, L-lysine is dissolved in a mixed solution of isopropanol and deionized water, and then tetraethyl orthosilicate is added at a rate of 15 drops / min, stirred for reaction for 2.5 hours, and then allowed to stand for 10 hours, wherein the molar ratio of tetraethyl orthosilicate, L-lysine, isopropanol, and deionized water is 1:0.02:2.5:230; subsequently, a fluorinated silane coupling agent and ethanol are added, and stirring is continued at 60° C. for 2 hours to obtain a modified silica sol, wherein the molar ratio of tetraethyl orthosilicate, the fluorinated silane coupling agent, and ethanol is 1:2:6. Example

[0024] A method for preparing antifouling hydrophobic photovoltaic glass, the preparation steps are as follows: (1) Pretreatment: The photovoltaic glass is placed in a 30% detergent solution with a volume 100 times its mass and ultrasonically cleaned for 30 minutes. After being taken out, it is rinsed with tap water until there are no bubbles. Then it is rinsed with deionized water until the conductivity of the rinsed water is close to that of deionized water. Then, the rinsed photovoltaic glass is immersed in a mixed solution of concentrated sulfuric acid and hydrogen peroxide, and ultrasonically oscillated at room temperature for 3 hours. After being taken out, it is repeatedly rinsed with deionized water and blown dry with nitrogen for later use to obtain the pretreated photovoltaic glass. The volume ratio of concentrated sulfuric acid to 60% hydrogen peroxide in the mixed solution of concentrated sulfuric acid and hydrogen peroxide is 4:9. (2) Primary coating: Spin coating the composite alumina sol onto the pretreated photovoltaic glass. The thickness of the spin coating liquid is adjusted to 250 μm by controlling the rotation speed and time of the turntable. After coating, the glass is placed in a muffle furnace and heated to 180°C and kept at this temperature for 4 h. The temperature is then raised to 450°C and kept at this temperature for 90 min. The furnace is allowed to cool naturally to room temperature, and the glass is taken out and then placed in deionized water at 95°C for hydrothermal treatment for 25 min. After the treatment, the glass is rinsed with deionized water and dried with nitrogen to obtain a photovoltaic glass with a primary coating. (3) Secondary coating: Spin-coat 250 μm modified nano-silica sol on the surface of the primary coated photovoltaic glass, then dry it in an electric oven at 80 °C for 30 min, and then anneal it in a muffle furnace for 2 h at a low temperature of 200 °C to obtain anti-fouling and hydrophobic photovoltaic glass; The preparation method of the composite alumina sol is as follows: under the stirring condition of 800 r / min, aluminum chloride is added to ethanol, wherein the mass ratio of ethanol to aluminum chloride is 8.4:1, then an ethylene glycol solution of polyvinyl pyrrolidone is added, and stirring and dissolving is continued, wherein the mass of polyvinyl pyrrolidone is 0.15 times the mass of aluminum chloride, and then a 0.1 mol / L silver nitrate solution is added, wherein the mass of silver nitrate is 0.075 times the mass of aluminum chloride, and stirring and mixing is continued for 20 minutes to obtain a composite alumina sol.

[0025] The preparation method of the modified silica sol is as follows: in a constant temperature water bath at 60° C. and under magnetic stirring, L-lysine is dissolved in a mixed solution of isopropanol and deionized water, and then tetraethyl orthosilicate is added at a rate of 20 drops / min, stirred for reaction for 3 hours, and then allowed to stand for 10 hours, wherein the molar ratio of tetraethyl orthosilicate, L-lysine, isopropanol, and deionized water is 1:0.03:2.5:300; subsequently, a fluorinated silane coupling agent and ethanol are added, and stirring is continued at 60° C. for 2 hours to obtain a modified silica sol, wherein the molar ratio of tetraethyl orthosilicate, the fluorinated silane coupling agent, and ethanol is 1:3:8.

[0026] Comparative Example 1 The difference between Comparative Example 1 and Example 2 is that aluminum isopropoxide is used to prepare the composite alumina sol, and the remaining steps and components are the same as those in Example 2.

[0027] Comparative Example 2 The difference between Comparative Example 2 and Example 2 is that the temperature is only raised once to 160° C. during the first coating, and the remaining steps and components are the same as those of Example 2.

[0028] Comparative Example 3 The difference between Comparative Example 3 and Example 2 is that the temperature is only raised once to 430° C. during the first coating, and the remaining steps and components are the same as those of Example 2.

[0029] Comparative Example 4 The difference between Comparative Example 4 and Example 2 is that alumina sol is used for the first coating, and the remaining steps and components are the same as those of Example 2.

[0030] Comparative Example 5 The only difference between Comparative Example 5 and Example 2 is that the composite alumina sol is prepared by adding silver nanowires to the alumina sol, and the remaining steps and components are the same as those in Example 2.

[0031] Comparative Example 6 The difference between Comparative Example 6 and Example 2 is that only composite alumina sol is used to coat the pretreated photovoltaic glass; the remaining steps and components are the same as those in Example 2.

[0032] Comparative Example 7 The difference between Comparative Example 7 and Example 2 is that only nano-silica sol is used for secondary coating; the remaining steps and components are the same as those of Example 2.

[0033] Comparative Example 8 The difference between Comparative Example 8 and Example 2 is that only modified nano-silica oxide sol is used to coat the pretreated photovoltaic glass; the remaining steps and components are the same as those in Example 2.

[0034] Effect example Light transmittance test: The antifouling and hydrophobic photovoltaic glass prepared in the embodiment and the comparative example was tested for light transmittance using a Hitachi U-4100 UV-visible-near infrared spectrophotometer (UV-VIS-NIR); Hydrophobicity: The water contact angle of the antifouling hydrophobic photovoltaic glass prepared in the embodiment and the comparative example was tested using a contact angle meter; Conductivity: The sheet resistance of the anti-fouling and hydrophobic photovoltaic glass surface prepared in the embodiment and the comparative example was measured using an RTS-9 dual-electrical four-probe tester; Film adhesion: The cross-hatch method is used to test the adhesion of the film on the surface of the anti-fouling and hydrophobic photovoltaic glass.

[0035] Table 1 below shows the performance test analysis results of the anti-fouling and hydrophobic photovoltaic glass prepared by Examples 1 to 3 of the present invention and Comparative Examples 1 to 8.

[0036] Table 1 Test items Light transmittance (%) Water contact angle (°) Sheet resistance (Ω / square) Adhesion (grade) Example 1 97.0 161.2 10.44 5B Example 2 97.1 163.8 10.04 5B Example 3 96.3 163.4 10.36 5B Comparative Example 1 71.8 141.4 68.43 3B Comparative Example 2 63.7 110.3 10.32 1B Comparative Example 3 72.3 144.5 68.62 2B Comparative Example 4 75.5 143.6 68.58 3B Comparative Example 5 96.4 136.7 67.84 1B Comparative Example 6 98.2 96.8 8.33 3B Comparative Example 7 96.5 145.6 10.24 5B Comparative Example 8 73.2 116.2 52.71 3B From Table 1, it can be found that the antifouling and hydrophobic photovoltaic glass prepared in the embodiment has strong antifouling and hydrophobic ability, good electrical conductivity, good surface adhesion and good light transmittance; compared with comparative examples 1, 4 and 5, it is found that the composite alumina sol prepared by using aluminum chloride, ethanol, ethylene glycol, polyvinyl pyrrolidone and silver nitrate solution has strong antifouling and hydrophobic ability, good electrical conductivity, good surface adhesion and good light transmittance; compared with comparative examples 2 to 3, it is found that the second stage of coating is performed once. When the temperature is raised, the antifouling and hydrophobic photovoltaic glass obtained has strong antifouling and hydrophobic ability, good electrical conductivity, good surface adhesion and good light transmittance; Compared with Comparative Examples 6 and 8, Example 2 shows that the antifouling and hydrophobic photovoltaic glass obtained by coating the pretreated photovoltaic glass with composite alumina sol and modified nano-silicon oxide sol in sequence has strong antifouling and hydrophobic ability, good electrical conductivity, good surface adhesion and good light transmittance; Compared with Comparative Example 7, Example 2 shows that the antifouling and hydrophobic photovoltaic glass obtained has strong antifouling and hydrophobic ability.

[0037] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

Claims

1. A method for preparing antifouling hydrophobic photovoltaic glass, characterized in that: The method comprises the following preparation steps: (1) Pretreatment: Place the photovoltaic glass in a 20-30% detergent solution with a concentration of 50-100 times its mass and ultrasonically clean it for 30 minutes. After taking it out, rinse it with tap water until there are no bubbles. Then rinse it with deionized water until the conductivity of the rinsed water is close to that of deionized water. Then immerse the rinsed photovoltaic glass in a mixed solution of concentrated sulfuric acid and hydrogen peroxide and ultrasonically oscillate it at room temperature for 1-3 hours. After taking it out, rinse it repeatedly with deionized water and blow it dry with nitrogen for later use to obtain the pretreated photovoltaic glass. (2) Primary coating: The composite alumina sol is applied to the pre-treated photovoltaic glass by spin coating, placed in a muffle furnace for two-stage heating treatment, and then subjected to hydrothermal treatment, followed by rinsing and drying to obtain a photovoltaic glass with a primary coating; (3) Secondary coating: Spin-coat the surface of the photovoltaic glass with the primary coating with modified silica sol, dry it for a period of time, and then anneal it at low temperature to obtain anti-fouling and hydrophobic photovoltaic glass.

2. The method for preparing the antifouling and hydrophobic photovoltaic glass according to claim 1, characterized in that: The volume ratio of the concentrated sulfuric acid to the 60% concentration hydrogen peroxide in the mixed solution of concentrated sulfuric acid and hydrogen peroxide is 4:

9.

3. The method for preparing the antifouling and hydrophobic photovoltaic glass according to claim 1, characterized in that: The preparation method of the composite alumina sol is as follows: under the stirring condition of 600-800 r / min, aluminum chloride is added to ethanol, wherein the mass ratio of ethanol to aluminum chloride is 8.2-8.4:1, then an ethylene glycol solution of polyvinyl pyrrolidone is added, and stirring and dissolving is continued, wherein the mass of polyvinyl pyrrolidone is 0.13-0.15 times the mass of aluminum chloride, and then a 0.1 mol / L silver nitrate solution is added, wherein the mass of silver nitrate is 0.065-0.075 times the mass of aluminum chloride, and stirring and mixing is continued for 20 minutes to obtain a composite alumina sol.

4. The method for preparing the antifouling and hydrophobic photovoltaic glass according to claim 1, characterized in that: The specific steps of the second stage heating are: heating to 140-180°C and keeping the temperature for 3-4 hours, and then continuing to heat to 400-450°C and keeping the temperature for 60-90 minutes.

5. The method for preparing antifouling and hydrophobic photovoltaic glass according to claim 1, characterized in that: The hydrothermal treatment temperature is 400-450° C., and the treatment time is 15-25 minutes.

6. The method for preparing antifouling and hydrophobic photovoltaic glass according to claim 1, characterized in that: The preparation method of modified silica sol is as follows: L-lysine is dissolved in a mixed solution of isopropanol and deionized water under a constant temperature water bath at 60°C and magnetic stirring, and then tetraethyl orthosilicate is added at a rate of 10-20 drops / min, stirred for reaction for 2-3 hours, and then allowed to stand for 10 hours, wherein the molar ratio of tetraethyl orthosilicate, L-lysine, isopropanol, and deionized water is 1:0.01-0.03:2.5:150-300; subsequently, a fluorinated silane coupling agent and ethanol are added, and stirring is continued at 60°C for 2 hours to obtain a modified silica sol, wherein the molar ratio of tetraethyl orthosilicate, fluorinated silane coupling agent, and ethanol is 1:1-3:5-8.

7. The method for preparing the antifouling and hydrophobic photovoltaic glass according to claim 6, characterized in that: The fluorine-containing silane coupling agent includes any one or more combinations of 1H,1H,2H,2H-perfluorodecyltriethoxysilane, 1H,1H,2H,2H-perfluorooctyltriethoxysilane, 1H,1H,2H,2H-perfluorooctyltrimethoxysilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, dodecafluoroheptylpropylmethyldimethoxysilane, dodecafluoroheptylpropyltrimethoxysilane, 3,3,3-trifluoropropylmethyldimethoxysilane, and 3.3,3-trifluoropropyltrimethoxysilane.

8. The method for preparing antifouling and hydrophobic photovoltaic glass according to claim 1, characterized in that: The drying temperature is 80° C. and the drying time is 30 minutes.

9. The method for preparing antifouling and hydrophobic photovoltaic glass according to claim 1, characterized in that: The low-temperature annealing temperature is 200° C. and the time is 2 hours.

10. The method for preparing antifouling and hydrophobic photovoltaic glass according to claim 1, characterized in that: The coating thickness of the composite alumina sol and the modified silica sol is 150-250 μm.