A low shrinkage cement paste material
By using a combination of modified nanosilicon dioxide and aramid nanofibers in cement slurry, nanomaterials with core-shell structures were prepared, which solved the problem of cracking in traditional cement-based materials in harsh environments, and achieved cement Low shrinkage and high mechanical properties improve the structural stability and durability of cement.
Patent Information
- Application Number
- CN202411337716.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-25
AI Technical Summary
Traditional cement-based materials are prone to cracks in harsh service environments, and the internal curing agents of high-performance cement materials such as nanocellulose gels have poor mechanical properties, which is difficult to meet the requirements of high-strength concrete, resulting in insufficient mechanical properties.
Using modified nanosilica and aramid nanofiber dispersion with core-shell structure, a cement slurry material with excellent shrinkage resistance and compressive strength is prepared by coating the combination of nanosilica and aramid fibers through PEO. , utilizes the nanosilica absorption and dispersion stress of core-shell structure to improve the mechanical properties of cement.
The low shrinkage and high mechanical properties of cement slurry are achieved, the compressive strength and water retention properties of cement are enhanced, and the structural stability and durability of cement are improved.
Smart Images

Figure CN118851649B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of cement-based materials, and in particular relates to a low-shrinkage cement paste material. Background Art
[0002] Cement-based materials are the basic materials for building all kinds of buildings, and the production of cement is a very polluting process. In the context of green production and construction, the requirements for cement production and the durability of cement materials are also urgently needed to be improved. On the one hand, the problem of global warming is becoming increasingly serious, and the demand for energy conservation and emission reduction in the production process of the cement industry is prominent. On the other hand, the structure of buildings is becoming more and more complex, and more and more buildings are in harsh service environments, which also puts higher requirements on the performance or function of cement-based materials.
[0003] Traditional cement-based materials are usually prone to cracks, especially in harsh service environments, which makes them easily restricted in actual engineering applications. Therefore, ordinary cement-based materials need to be modified to improve their strength and durability. The composition, structure and performance of cement-based materials are closely related and influence each other. In order to obtain macro-technical performance that meets engineering requirements, it is necessary to optimize the material composition design under the premise that the quality of raw materials meets the requirements. The microstructure of cement materials is the fundamental factor of their macro-performance.
[0004] At present, cement prefabricated component factories often use rapid curing methods, such as electric heat curing, moist heat curing, dry heat curing, high-frequency electric heat curing, infrared curing, hot air curing, electromagnetic field curing, hot mix and hot vibration concrete curing, and steam curing, etc. If the curing method is used correctly, it can significantly improve the initial and early strength of cement, speed up mold turnover, shorten the production cycle, and improve production efficiency.
[0005] However, with the development of cement-based material related technologies, especially the widespread application of low water-cement ratio cement-based materials represented by high-performance cement and ultra-high performance cement, due to its dense structure, traditional maintenance has just highlighted disadvantages. Most of the prior art uses superabsorbent resin and nanocellulose gel as internal curing agent. For example, patents such as CN111892378A, CN112321213A, and CN 116120018A all use nanocellulose as gel frame for mortar field. However, nanocellulose gel has poor mechanical properties and is difficult to meet the use requirements of high-strength concrete. It is mainly used in the field of thermal insulation mortar. Although CN116694126A prepares aramid nanofiber aerogel, it adopts in-situ polymerization process to prepare aramid nanofiber, and the fiber aspect ratio formed is small, and the mechanical properties are poor. The mechanical strength of the prepared aerogel is low, and it can only be applied to the field of low-strength thermal insulation putty to achieve the technical effect of thermal insulation. Therefore, how to improve these existing maintenance problems and improve the mechanical properties of cement on the basis of preventing cement shrinkage and cracking has become the focus and hot spot of current research. Summary of the invention
[0006] Based on the above content, the present invention provides a low shrinkage cement paste material. The present invention can reduce the shrinkage rate of cement paste and improve the mechanical properties of cement paste.
[0007] To achieve the above object, the present invention provides the following solutions:
[0008] A low shrinkage cement paste material, wherein the mass ratio of cement to internal curing agent in the cement paste is 100:(0.1-2);
[0009] The preparation method of the internal curing agent comprises the following steps:
[0010] (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared;
[0011] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silica is 100:(1-15);
[0012] (3) adding modified nano-silica to the aramid nanofiber dispersion, dispersing by ultrasonication, and then adding deionized water to obtain a mixed solution;
[0013] (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel;
[0014] (5) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0015] Although the aramid nanofibers prepared by the alkali / DMSO immersion method have a large aspect ratio and excellent mechanical properties, they are prone to fiber bundle merging in aqueous solution, resulting in fiber agglomeration, which affects the porosity and water retention of the gel. Moreover, as an organic gel material, the aramid nanofiber gel will shrink in volume after releasing water, which seriously affects the safety, stability and durability of the structure. In order to improve the structural stability of the gel, the present invention first adds polymer-coated silica to the mixed solution of alkali and dimethyl sulfoxide of the aramid nanofibers, and then adds water; compared with first adding water to the aramid nanofiber dispersion and then adding polymer-coated silica, the dispersion performance of the nanofibers can be more effectively improved. Furthermore, the mass ratio of aramid fiber to modified nano-silica is 100: (6-10); the introduction of an appropriate amount of polymer-coated silica not only disperses the stress on the gel and enhances the mechanical properties of the gel; but also plays a role in enhancing the mechanical strength of the gel framework, thereby improving the mechanical properties and shrinkage resistance of the cement paste.
[0016] In previous work, the inventor used inorganic nanoparticles modified with coupling agents as reinforcing and modifying agents for aramid fibers. Although the water absorption and water loss stability of the internal curing agent were improved to a certain extent, the above process was complicated, the inorganic particles had poor compatibility with aramid nanofibers, and the mechanical strength of the gel network was reduced. More importantly, directly using inorganic nanoparticles as reinforcing and modifying agents for aramid fibers will affect the flow properties of cement. Cement paste is usually required to have high fluidity, which is used to fill or seal cracks, or as an adhesive during construction to ensure its firm connection. Due to the poor control of the proportion of cement paste components, improper operation can easily lead to unsatisfactory performance of the repaired concrete structure.
[0017] The present invention prepares PEO-coated silicon dioxide nanoparticles with the assistance of a surfactant. Polyethylene oxide molecules contain a large number of oxygen atoms, which can form hydrogen bonds, making the polyethylene oxide molecules highly hydrophilic and promoting the dispersion of inorganic nanoparticles in a solution; and when polyethylene oxide contacts water, due to the polarity of the polyethylene oxide molecule surface, water molecules can interact with it, thereby forming hydrogen bonds with polyethylene oxide, so that polyethylene oxide plays the role of a surfactant, promoting the dispersion of silicon dioxide nanoparticles in aramid nanofibers, and also inhibiting the agglomeration between aramid nanofibers. Moreover, the introduction of the flexible coating layer effectively disperses the stress on the cement matrix, and is added to the cement slurry as a damping filler to form a microscopic constrained damping structure inside the cement slurry, which can promote the dissipation of cement matrix energy and retain the mechanical strength of the cement matrix on the basis of exerting the water retention performance of the internal curing agent.
[0018] Furthermore, the preparation process of the modified nano-silicon dioxide in step (1) is:
[0019] S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion;
[0020] S2, dissolving PEO in deionized water to obtain a PEO solution, and adding the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 2-5 hours;
[0021] S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
[0022] Furthermore, in step S1, the particle size of the nano-silicon dioxide particles is 50-500 nm.
[0023] Furthermore, in step S1, the surfactant is one or more of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate.
[0024] Furthermore, in step S2, the stirring rate is 500-600 r / min.
[0025] Furthermore, in the preparation process of the modified nano-silica, the mass ratio of nano-silica, surfactant and PEO is 1: (0.05-0.2): (0.2-0.8).
[0026] Furthermore, in step (2), the alkali is sodium hydroxide or potassium hydroxide; the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1 g: (1-2) g: (400-500) mL; and the stirring is performed at room temperature for 4-8 days.
[0027] Furthermore, in step (3), the frequency of ultrasonic dispersion is 50-70 kHz; and the ratio of aramid fiber to deionized water is 1 g: (250-300) mL.
[0028] Furthermore, in step (4), the steam bath is an acetic acid steam bath or a hydrochloric acid steam bath, and the steam bath treatment time is 7-9 hours.
[0029] Furthermore, the cement paste also includes water and a water reducing agent. The mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100: (0.1-2): (0.1-1): (35-50).
[0030] Beneficial effects:
[0031] 1. The cement paste prepared by the present invention using specific raw materials and proportions has excellent anti-shrinkage performance and compressive strength.
[0032] 2. The present invention uses a specific core-shell structure of nano-silicon dioxide as a reinforcing agent for aramid nanofiber gel, which not only plays a role of isolation and reinforcement, but also the flexible shell can absorb and release the stress inside the cement-based material, and the rigid internal core plays a role in maintaining the strength of the matrix. When subjected to external force, the core-shell structure of nano-silicon dioxide can effectively absorb and disperse the stress, prevent stress concentration, and improve the mechanical properties of cement.
[0033] 3. The free water absorbed by the internal curing agent used in the present invention exerts an internal curing effect on cement to reduce autogenous shrinkage and compensate for the strength reduction phenomenon caused by the drying collapse of the gel. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a scanning electron microscope image of the modified nano-silicon dioxide prepared in Example 6;
[0035] Figure 2 This is a transmission electron microscopy image of the modified nano-silicon dioxide prepared in Example 6;
[0036] Figure 3 This is a test chart of the water retention performance of the internal curing agent prepared in Examples 1-5;
[0037] Figure 4 This is a test chart of the water retention performance of the internal curing agent prepared in Examples 6-8 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Among them, the aramid fiber used in the embodiments of the present invention and the comparative example is DuPont Kevlar fiber; the particle size of the nano-silicon dioxide particles is 200nm; the surfactant is sodium dodecyl sulfate; and the cement is silicate cement.
[0039] Example 1
[0040] A low shrinkage cement paste material, wherein the mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100:0.5:0.1:40;
[0041] The preparation method of the internal curing agent comprises the following steps:
[0042] (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared;
[0043] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing an aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silicon dioxide is 100:6; the alkali is potassium hydroxide; the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1g:1g:400mL; stirring is stirring at room temperature for 4 days;
[0044] (3) Adding modified nano-silica to the aramid nanofiber dispersion, ultrasonically dispersing, and then adding deionized water to obtain a mixed solution; the frequency of ultrasonic dispersion is 60 kHz; the ratio of aramid fiber to deionized water is 1 g: 250 mL;
[0045] (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; the steam bath is a hydrochloric acid steam bath, and the steam bath treatment time is 8 hours;
[0046] (5) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0047] The preparation process of modified nano-silicon dioxide in step (1) is:
[0048] S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion;
[0049] S2, dissolving PEO in deionized water to obtain a PEO solution, and adding the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 3 hours; the stirring rate is 500r / min; the mass ratio of nano-silicon dioxide, surfactant, and PEO is 1:0.05:0.2;
[0050] S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
[0051] Example 2
[0052] A low shrinkage cement paste material, wherein the mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100:2:1:40;
[0053] The preparation method of the internal curing agent comprises the following steps:
[0054] (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared;
[0055] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing an aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silicon dioxide is 100:10; the alkali is potassium hydroxide; the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1g:2g:500mL; stirring is stirring at room temperature for 7 days;
[0056] (3) Adding modified nano-silica to the aramid nanofiber dispersion, ultrasonically dispersing, and then adding deionized water to obtain a mixed solution; the frequency of ultrasonic dispersion is 60 kHz; the ratio of aramid fiber to deionized water is 1 g: 300 mL;
[0057] (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; the steam bath is an acetic acid steam bath, and the steam bath treatment time is 8 hours;
[0058] (5) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0059] The preparation process of modified nano-silicon dioxide in step (1) is:
[0060] S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion;
[0061] S2, dissolving PEO in deionized water to obtain a PEO solution, and adding the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 3 hours; the stirring rate is 500r / min; the mass ratio of nano-silicon dioxide, surfactant, and PEO is 1:0.2:0.8;
[0062] S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
[0063] Example 3
[0064] A low shrinkage cement paste material, wherein the mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100:0.7:1:40;
[0065] The preparation method of the internal curing agent comprises the following steps:
[0066] (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared;
[0067] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing an aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silicon dioxide is 100:10; the alkali is potassium hydroxide; the ratio of aramid fiber, alkali and dimethyl sulfoxide is 1g:2g:400mL; stirring is stirring at room temperature for 5 days;
[0068] (3) Adding modified nano-silica to the aramid nanofiber dispersion, ultrasonically dispersing, and then adding deionized water to obtain a mixed solution; the frequency of ultrasonic dispersion is 60 kHz; the ratio of aramid fiber to deionized water is 1 g: 300 mL;
[0069] (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; the steam bath is an acetic acid steam bath, and the steam bath treatment time is 8 hours;
[0070] (5) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0071] The preparation process of modified nano-silicon dioxide in step (1) is:
[0072] S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion;
[0073] S2, dissolving PEO in deionized water to obtain a PEO solution, and adding the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 3 hours; the stirring rate is 500r / min; the mass ratio of nano-silicon dioxide, surfactant, and PEO is 1:0.2:0.2;
[0074] S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
[0075] Example 4
[0076] A low shrinkage cement paste material, wherein the mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100:0.5:0.1:40;
[0077] The preparation method of the internal curing agent comprises the following steps:
[0078] (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared;
[0079] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing an aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silicon dioxide is 100:9; the alkali is potassium hydroxide; the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1g:1g:500mL; stirring is stirring at room temperature for 5 days;
[0080] (3) Adding modified nano-silica to the aramid nanofiber dispersion, ultrasonically dispersing, and then adding deionized water to obtain a mixed solution; the frequency of ultrasonic dispersion is 60 kHz; the ratio of aramid fiber to deionized water is 1 g: 300 mL;
[0081] (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; the steam bath is an acetic acid steam bath, and the steam bath treatment time is 8 hours;
[0082] (5) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0083] The preparation process of modified nano-silicon dioxide in step (1) is:
[0084] S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion;
[0085] S2. Dissolve PEO in deionized water to obtain a PEO solution, and add the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 3 hours; the stirring rate is 500r / min; the mass ratio of nano-silicon dioxide, surfactant, and PEO is 1:0.06:0.7;
[0086] S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
[0087] Example 5
[0088] A low shrinkage cement paste material, wherein the mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100:1.2:0.3:40;
[0089] The preparation method of the internal curing agent comprises the following steps:
[0090] (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared;
[0091] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing an aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silicon dioxide is 100:7; the alkali is potassium hydroxide; the ratio of aramid fiber, alkali and dimethyl sulfoxide is 1g:1.7g:420mL; stirring is stirring at room temperature for 7 days;
[0092] (3) Adding modified nano-silica to the aramid nanofiber dispersion, ultrasonically dispersing, and then adding deionized water to obtain a mixed solution; the frequency of ultrasonic dispersion is 60 kHz; the ratio of aramid fiber to deionized water is 1 g: 300 mL;
[0093] (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; the steam bath is a hydrochloric acid steam bath, and the steam bath treatment time is 8 hours;
[0094] (5) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0095] The preparation process of modified nano-silicon dioxide in step (1) is:
[0096] S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion;
[0097] S2. Dissolve PEO in deionized water to obtain a PEO solution, and add the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 3 hours; the stirring rate is 500r / min; the mass ratio of nano-silicon dioxide, surfactant, and PEO is 1:0.08:0.6;
[0098] S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
[0099] Example 6
[0100] A low shrinkage cement paste material, wherein the mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100:1:0.6:40;
[0101] The preparation method of the internal curing agent comprises the following steps:
[0102] (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared;
[0103] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing an aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silicon dioxide is 100:8; the alkali is potassium hydroxide; the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1g:1.4g:450mL; stirring is performed at room temperature for 6 days;
[0104] (3) Adding modified nano-silica to the aramid nanofiber dispersion, ultrasonically dispersing, and then adding deionized water to obtain a mixed solution; the frequency of ultrasonic dispersion is 60 kHz; the ratio of aramid fiber to deionized water is 1 g: 300 mL;
[0105] (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; the steam bath is an acetic acid steam bath, and the steam bath treatment time is 8 hours;
[0106] (5) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0107] The preparation process of modified nano-silicon dioxide in step (1) is:
[0108] S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion;
[0109] S2. Dissolve PEO in deionized water to obtain a PEO solution, and add the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 3 hours; the stirring rate is 500r / min; the mass ratio of nano-silicon dioxide, surfactant, and PEO is 1:0.1:0.5;
[0110] S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
[0111] Example 7
[0112] A low shrinkage cement paste material, wherein the mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100:1:0.6:40;
[0113] The preparation method of the internal curing agent comprises the following steps:
[0114] (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared;
[0115] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing an aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silicon dioxide is 100:1; the alkali is potassium hydroxide; the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1g:1.4g:450mL; stirring is stirring at room temperature for 6 days;
[0116] (3) Adding modified nano-silica to the aramid nanofiber dispersion, ultrasonically dispersing, and then adding deionized water to obtain a mixed solution; the frequency of ultrasonic dispersion is 60 kHz; the ratio of aramid fiber to deionized water is 1 g: 300 mL;
[0117] (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; the steam bath is an acetic acid steam bath, and the steam bath treatment time is 8 hours;
[0118] (5) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0119] The preparation process of modified nano-silicon dioxide in step (1) is:
[0120] S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion;
[0121] S2. Dissolve PEO in deionized water to obtain a PEO solution, and add the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 3 hours; the stirring rate is 500r / min; the mass ratio of nano-silicon dioxide, surfactant, and PEO is 1:0.1:0.5;
[0122] S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
[0123] Example 8
[0124] A low shrinkage cement paste material, wherein the mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100:1:0.6:40;
[0125] The preparation method of the internal curing agent comprises the following steps:
[0126] (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared;
[0127] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing an aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silicon dioxide is 100:15; the alkali is potassium hydroxide; the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1g:1.4g:450mL; stirring is performed at room temperature for 6 days;
[0128] (3) Adding modified nano-silica to the aramid nanofiber dispersion, ultrasonically dispersing, and then adding deionized water to obtain a mixed solution; the frequency of ultrasonic dispersion is 60 kHz; the ratio of aramid fiber to deionized water is 1 g: 300 mL;
[0129] (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; the steam bath is an acetic acid steam bath, and the steam bath treatment time is 8 hours;
[0130] (5) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0131] The preparation process of modified nano-silicon dioxide in step (1) is:
[0132] S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion;
[0133] S2. Dissolve PEO in deionized water to obtain a PEO solution, and add the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 3 hours; the stirring rate is 500r / min; the mass ratio of nano-silicon dioxide, surfactant, and PEO is 1:0.1:0.5;
[0134] S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
[0135] Comparative Example 1
[0136] A low shrinkage cement paste material, wherein the mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100:1:0.6:40;
[0137] The preparation method of the internal curing agent comprises the following steps:
[0138] (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared;
[0139] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing an aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silicon dioxide is 100:8; the alkali is potassium hydroxide; the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1g:1.4g:450mL; stirring is performed at room temperature for 6 days;
[0140] (3) adding water to the aramid nanofiber dispersion to dilute it, and then adding modified nano-silica and ultrasonically dispersing it to obtain a mixed solution; the frequency of ultrasonic dispersion is 60 kHz; the ratio of aramid fiber to deionized water is 1 g: 300 mL;
[0141] (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; the steam bath is an acetic acid steam bath, and the steam bath treatment time is 8 hours;
[0142] (5) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0143] The preparation process of modified nano-silicon dioxide in step (1) is:
[0144] S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion;
[0145] S2. Dissolve PEO in deionized water to obtain a PEO solution, and add the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 3 hours; the stirring rate is 500r / min; the mass ratio of nano-silicon dioxide, surfactant, and PEO is 1:0.1:0.5;
[0146] S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
[0147] Comparative Example 2
[0148] A low shrinkage cement paste material, wherein the mass ratio of cement, internal curing agent, water reducing agent and water in the cement paste is 100:1:0.6:40;
[0149] The preparation method of the internal curing agent comprises the following steps:
[0150] (1) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing an aramid nanofiber dispersion; the mass ratio of aramid fiber to nano-silicon dioxide is 100:8; the alkali is potassium hydroxide; the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1g:1.4g:450mL; stirring is performed at room temperature for 6 days;
[0151] (2) Adding nano-silicon dioxide to the aramid nanofiber dispersion, ultrasonically dispersing, and then adding deionized water to obtain a mixed solution; the frequency of ultrasonic dispersion is 60 kHz; the ratio of aramid fiber to deionized water is 1 g: 300 mL;
[0152] (3) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; the steam bath is an acetic acid steam bath, and the steam bath treatment time is 8 hours;
[0153] (4) The hydrogel is freeze-dried and crushed to obtain an internal curing agent.
[0154] The mechanical properties of cement paste were tested according to GB / T 50081-2019; the shrinkage of cement paste was tested according to GB / T 50082-2009. The weight of the internal curing agent that reached water absorption equilibrium was recorded as W 0 Then place the internal curing agent that has reached water absorption equilibrium in a room temperature environment and weigh its weight W after 1 day, 2 days, 3 days...10 days. d The water retention rate of the internal curing agent is calculated by the following formula: Water retention rate = (W d / W 0 )×100%.
[0155]
[0156] Figure 1 and Figure 2 They are scanning electron microscope images and transmission electron microscope images of the modified nano-silica prepared in Example 6, respectively; it can be seen from the figures that the present invention successfully prepared PEO-coated nano-silica particles. Figure 3-Figure 4 The water retention performance test diagram of the internal curing agent prepared in Examples 1-8 and Comparative Examples 1-2. It can be seen from the figure that the polyethylene oxide coating layer in the PEO-coated silica nanoparticles has a strong hydrophilicity, which promotes the dispersion of inorganic nanoparticles in the solution; and when polyethylene oxide comes into contact with water, due to the polarity of the polyethylene oxide molecule surface, water molecules will interact with it, thereby forming hydrogen bonds with polyethylene oxide, so that polyethylene oxide plays the role of a surfactant, promotes the dispersion of silica nanoparticles in aramid nanofibers, and also inhibits the agglomeration phenomenon between aramid nanofibers, thereby improving the water retention performance of the gel.
[0157] As can be seen from Table 1 and Table 2, the present invention uses a specific core-shell structure of nano-silica as a reinforcing agent for aramid nanofiber gel, which not only plays a role of isolation and reinforcement, but also the flexible shell can absorb and release the stress inside the cement-based material, and the rigid internal core plays a role in maintaining the strength of the matrix. When subjected to external force, the core-shell structure of nano-silica can effectively absorb and disperse the stress, prevent stress concentration, and improve the mechanical properties of cement. Compared with Example 6, Comparative Example 1 is different only in the order of adding coated nanoparticles and deionized water. Deionized water is first added to the aramid nanofiber dispersion. Due to the lack of isolation of coated nanoparticles, it is easy to cause fiber agglomeration, affecting the performance of the curing agent. Compared with Example 6, Comparative Example 2 does not coat nano-silica, and the hydrophilicity of the particles is reduced, which affects the water retention performance of the gel; and the function of absorbing and dispersing stress of the core-shell structure of nano-silica is lost, resulting in reduced mechanical properties of cement slurry.
[0158] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A low shrinkage cement paste material, characterized in that: The mass ratio of cement to internal curing agent in cement paste is 100:(0.1-2); The preparation method of the internal curing agent comprises the following steps: (1) Using PEO as the shell and nano-silica as the core, modified nano-silica with a core-shell structure was prepared; (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, stirring evenly, and preparing aramid nanofiber dispersion; the mass ratio of aramid fiber to modified nano-silica is 100:(1-15); (3) adding modified nano-silica to the aramid nanofiber dispersion, dispersing by ultrasonication, and then adding deionized water to obtain a mixed solution; (4) preparing an initial hydrogel by subjecting the mixed solution to a steam bath; and exchanging the solvent of the initial hydrogel with deionized water to obtain a hydrogel; (5) freeze-drying the hydrogel and crushing it to obtain an internal curing agent; The steam bath in step (4) is an acetic acid steam bath or a hydrochloric acid steam bath.
2. A low shrinkage cement paste material as claimed in claim 1, characterized in that: The preparation process of modified nano-silicon dioxide in step (1) is: S1, dispersing nano-silicon dioxide and a surfactant in deionized water to obtain a nano-silicon dioxide dispersion; S2, dissolving PEO in deionized water to obtain a PEO solution, and adding the PEO solution dropwise to the nano-silicon dioxide dispersion while stirring; after the addition is completed, continue stirring for 2-5 hours; S3, centrifuging, washing and drying the reaction solution to obtain modified nano-silica.
3. A low shrinkage cement paste material as claimed in claim 2, characterized in that: In step S1, the particle size of the nano-silicon dioxide is 50-500 nm.
4. A low shrinkage cement paste material as claimed in claim 2, characterized in that: In step S1, the surfactant is one or more of sodium dodecyl sulfate and sodium dodecylbenzene sulfonate.
5. A low shrinkage cement paste material as claimed in claim 2, characterized in that: The stirring rate in step S2 is 500-600 r / min.
6. A low shrinkage cement paste material as claimed in claim 2, characterized in that: In the preparation process of the modified nano-silicon dioxide, the mass ratio of nano-silicon dioxide, surfactant and PEO is 1: (0.05-0.2): (0.2-0.8).
7. A low shrinkage cement paste material as claimed in claim 1, characterized in that: In the step (2), the alkali is sodium hydroxide or potassium hydroxide; the ratio of the aramid fiber, the alkali and the dimethyl sulfoxide is 1 g: (1-2) g: (400-500) mL; and the stirring is carried out at room temperature for 4-8 days.
8. The low shrinkage cement paste material according to claim 1, characterized in that: The frequency of ultrasonic dispersion in step (3) is 50-70 kHz; the ratio of aramid fiber to deionized water is 1 g: (250-300) mL.
9. The low shrinkage cement paste material according to claim 1, characterized in that: In the step (4), the steam bath treatment time is 7-9 hours.