A low-temperature heavy-duty foam tape and preparation method thereof

By coating acrylic polymer and pressure-sensitive adhesive layers on foam tape and leveraging the high shrinkage characteristics under low temperature conditions, the problem of damage to parts and process complexity in existing foam tape during heavy industry is solved, and the problem of failure of parts and process in real time is achieved without Easy rework of residual glue and debris-free reduces cost and complexity.

CN115746732BActive Publication Date: 2024-12-06SUZHOU SHIHUA NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211525635.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-12-06
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

The existing heavy-industrial foam tape needs to be violently removed during heavy-industrial processes, which can easily damage parts and be complex in process, high in cost, and produce foam debris, which limits its application scope.

Method used

Using low-temperature heavy-industrial foam tape, the substrate is coated with acrylic polymer coating and pressure-sensitive adhesive layer on both sides, and the release film is bonded to the outside, so as to utilize the high shrinkage characteristics of acrylic pressure-sensitive adhesive under low temperature conditions. No residue reworking, avoid degumming and foam debris.

Benefits of technology

It realizes easy rework without residual glue, degumming and foam debris under low temperature conditions, reducing process complexity and cost, expanding application scope, and protecting parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003973465010000141
    Figure BDA0003973465010000141
Patent Text Reader

Abstract

The present invention relates to the technical field of tape production, and specifically to a foam tape for low-temperature rework and a preparation method thereof. The present invention mainly contains primary amine groups in the side chains and acrylic polymers in the main chains, and is combined with epoxy compounds, isocyanates or metal salt crosslinkers to prepare an acrylic polymer coating with excellent adhesion at low temperatures. The coating has good adhesion to various foam substrates, and has excellent shrinkage resistance, low temperature resistance and weather resistance. By using acrylic pressure-sensitive adhesive, tackifying resin, and selecting polyisocyanates, epoxy curing agents or metal salt curing agents as curing agents, a pressure-sensitive adhesive layer is prepared, so that the pressure-sensitive adhesive layer has high shrinkage characteristics under low temperature conditions, and can lose adhesion and separate from the adhered object when subjected to external force. The foam tape for low-temperature rework prepared by the present invention has no residual glue and degumming during the rework process, and no foam debris is generated, and there is no damage to the parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesive tape production, in particular to a low-temperature heavy-duty foam adhesive tape and a preparation method thereof. Background Art

[0002] In recent years, the update speed of electronic products such as mobile phones, computers, and televisions has become faster and faster, and they tend to be thinner, with narrow frames and no frames. In order to better bond and fix different electronic components, the application of foam tapes has become more and more extensive. Among them, reworkable foam tapes have been widely used in the consumer electronics field such as smart phones, tablet computers, large-size LCDs and other products due to their excellent buffering, sealing, waterproof, dustproof, flame retardant and removable properties. It can be used for bonding LCD display modules and backlight modules, bonding LCD frames, and bonding LCD modules and back shells.

[0003] When repairing or reworking these parts, traditional reworkable foam tapes need to be violently removed from the front or cut the foam in the middle with a knife and then remove the remaining tape by stretching. Due to the limitation of its rework method, its application occasions are greatly limited and can only be used in places that are convenient to cut directly with a knife, such as bonding the frame of a TV. The foam debris generated during the rework process will contaminate some precision parts and easily cause damage to the parts. In addition, the existing reworkable foam double-sided adhesives mainly use hot pressing or specific glue to combine stretchable films with foam as the base material, which is complex and costly.

[0004] Therefore, providing a product that has a wide range of applications, simple process, low cost, fast rework without residue, and can replace foam double-sided tape in the field of large-size module bonding and can remove double-sided tape has become a technical problem that needs to be urgently solved by technical personnel in this field.

[0005] In order to solve the above problems, the present invention provides a low-temperature heavy-duty foam tape and a preparation method thereof. Summary of the invention

[0006] The object of the present invention is to provide a low temperature heavy duty foam tape and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] A low-temperature reworkable foam tape, the foam tape comprising a substrate, the substrate being a foam substrate coated with an acrylic polymer coating on both sides, a pressure-sensitive adhesive layer attached to one side or both sides of the substrate, and a release film attached to the outer side of the pressure-sensitive adhesive layer;

[0009] The acrylic polymer coating is mainly composed of an acrylic polymer coating having a primary amine group in the side chain.

[0010] Preferably, the acrylic polymer coating is composed of the following ingredients:

[0011] 100 parts of acrylic polymer containing primary amine groups in the side chains;

[0012] 1-5 parts of curing agent;

[0013] 300-500 parts of solvent;

[0014] The acrylic polymer containing primary amino groups in the side chain is mainly obtained by free radical polymerization of low shrinkage acrylic monomer and benzyloxycarbonyl protected amino acrylic monomer under the action of an initiator;

[0015] The side chain of the acrylic polymer contains primary amino groups, the content ratio of amino groups to acrylic acid solids is 0.5-1.5 mmol / g, the viscosity is 500-2000 mPa·s / 25°C, the glass transition temperature is -40-50°C, the weight average molecular weight is 50000-200000, and the molecular weight is 1.8-3.5.

[0016] More optimally, the curing agent is any one or more of polyisocyanate, epoxy curing agent, and metal salt curing agent.

[0017] Preferably, the side chain of the acrylic polymer containing primary amine groups is composed of the following components: by weight:

[0018] 75-85 parts of low shrinkage acrylic monomer;

[0019] 15-20 parts of benzyloxycarbonyl protected aminoacrylic acid monomer;

[0020] Thermal initiator 0.1-0.5 parts;

[0021] 80-150 parts of solvent.

[0022] More optimally, the low-shrinkage acrylic monomer is any one or more of 4-tert-butyl cyclohexyl acrylate, stearic acid methacrylate, lauric acid methacrylate, ethoxyethoxyethyl acrylate, isotridecyl methacrylate, and octadecyl acrylate; the benzyloxycarbonyl-protected amino acrylic monomer is any one or more of methacrylate-2-(benzyloxycarbonylamino)ethyl ester and acrylate-2-(benzyloxycarbonylamino)ethyl ester; the thermal initiator is any one or more of azobisisobutyronitrile, azobisisoheptylnitrile, benzoyl peroxide, lauroyl peroxide, and tert-butyl perbenzoate.

[0023] Preferably, the pressure-sensitive adhesive layer is composed of the following components: by weight:

[0024] 100 parts of acrylic pressure-sensitive adhesive;

[0025] 5-30 parts of tackifying resin;

[0026] 1-5 parts of black color paste;

[0027] Curing agent 0.2-3 parts;

[0028] 50-200 parts of solvent;

[0029] The acrylic pressure-sensitive adhesive has a glass transition temperature of -20-10°C, a weight-average molecular weight of 350,000-850,000, and a molecular weight distribution of 1.4-3.; the storage modulus of the acrylic pressure-sensitive adhesive at -40°C is 350,000-750,000 KPa, and the loss factor is 0.05-0.11; the storage modulus of the acrylic pressure-sensitive adhesive at 23°C is 80-200 KPa, and the loss factor is 0.8-1.35; the storage modulus of the acrylic pressure-sensitive adhesive at 85°C is 10-50 KPa, and the loss factor is 0.25-0.75; and the softening point is 75-1560°C.

[0030] More optimally, the tackifying resin is any one or more of rosin resin, modified rosin resin, terpene resin and petroleum resin; the curing agent is any one or more of polyisocyanate, epoxy curing agent and metal salt curing agent.

[0031] Preferably, the thickness of the substrate is 0.05-3 mm;

[0032] The thickness of the pressure-sensitive adhesive layer is 5-100 μm;

[0033] The release film has a thickness of 50-100 μm;

[0034] The substrate is any one or more of polyurethane foam, polyethylene foam, and polypropylene foam.

[0035] A method for preparing a low-temperature heavy-duty foam tape comprises the following steps:

[0036] Step 1: Take a low-shrinkage acrylic monomer, a benzyloxycarbonyl-protected amino acrylic monomer, a thermal initiator, and a solvent, mix them evenly, react at 65-90° C. for 6-10 hours, add a hydrogen bromide acetic acid solution to deprotect the amino group, and obtain an acrylic polymer containing a primary amino group in the side chain;

[0037] Step 2: Take an acrylic polymer having a primary amine group in the side chain, a curing agent, and a solvent, mix them evenly to obtain an acrylic polymer; apply the acrylic polymer on both sides of the foam substrate, and dry at 90-120° C. for 3-10 minutes to obtain an acrylic polymer coating;

[0038] Step 3: Mixing and stirring the acrylic pressure-sensitive adhesive, tackifying resin, black color paste, curing agent, and solvent, and ultrasonically dispersing the mixture to obtain a pressure-sensitive adhesive;

[0039] Step 4: coating a pressure-sensitive adhesive on the release surface of the release film, drying the pressure-sensitive adhesive layer, and laminating the pressure-sensitive adhesive layer on a foam substrate to obtain a low-temperature reworkable foam tape.

[0040] More optimally, the preparation method of the benzyloxycarbonyl protected aminoacrylic acid monomer is: take deionized water, ether, aminoacrylic acid monomer, and alkaline reagent, stir evenly, drop benzyl chloroformate, stir, add glycine, stir and react for 19-21 hours, wash, dry, filter, concentrate the filtrate by rotary evaporation, and vacuum dry to obtain the benzyloxycarbonyl protected aminoacrylic acid monomer;

[0041] The aminoacrylic acid monomer is any one or more of 2-aminoethyl methacrylate and 2-aminoethyl acrylate; the alkaline reagent is any one or more of sodium carbonate, potassium carbonate, sodium bicarbonate and sodium hydroxide.

[0042] More optimally, the coating method is any one of micro-concave coating and comma blade coating.

[0043] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0044] (1) The present invention mainly contains primary amine groups in the side chain and acrylic polymer in the main chain, and is combined with epoxy compounds, isocyanates or metal salt crosslinking agents to react with the foam substrate and retain certain reactive groups on the surface of the substrate so that it can react with the acrylic pressure-sensitive adhesive to form an acrylic polymer coating with excellent adhesion at low temperatures. The coating has good adhesion to various foam substrates, excellent shrinkage resistance, low temperature resistance and weather resistance, and will not separate from the substrate and the acrylic adhesive layer even at -78°C, ensuring that the adhesive layer will not fall off from the substrate under low temperature conditions.

[0045] By controlling the raw materials and the addition amount of the pressure-sensitive adhesive layer, an acrylic pressure-sensitive adhesive with a glass transition temperature of -20-10°C, a weight average molecular weight of 350,000-850,000, and a molecular weight distribution of 1.4-3.2 is used; the storage modulus of the acrylic pressure-sensitive adhesive at -40°C is 350,000-750,000 KPa, and the loss factor is 0.05-0.11; the storage modulus of the acrylic pressure-sensitive adhesive at 23°C is 80-200 KPa, and the loss factor is 0 .8-1.35; the storage modulus of the acrylic pressure-sensitive adhesive at 85°C is 10-50KPa, and the loss factor is 0.25-0.75; the softening point is 75-1560°C, the molecular weight distribution is concentrated, the bonding with the substrate is good, and the temperature resistance is good. The tackifying resin is selected as polyisocyanate, epoxy curing agent and metal salt curing agent as curing agent to prepare the pressure-sensitive adhesive layer, so that the pressure-sensitive adhesive layer has high shrinkage characteristics under low temperature conditions, and can lose adhesion and separate from the adhered object when subjected to external force.

[0046] The low-temperature rework foam tape prepared by the present invention utilizes the high shrinkage property of the acrylic pressure-sensitive adhesive layer under low-temperature conditions. When subjected to external force, it can lose adhesion and separate from the adhered object to achieve rework. The good adhesion and low-temperature resistance and low shrinkage property of the acrylic polymer at low temperatures can ensure the bonding between the adhesive layer and the foam substrate, so that no debonding or residual glue occurs in this process. When reworking the low-temperature rework foam tape prepared by the present invention, it is only necessary to put the parts that need to be reworked or repaired into a refrigeration device below -40°C, then take out the parts that are bonded together and gently separate them, and remove the tape from the parts after returning to room temperature. During the whole process, there is no residual glue and debonding, no foam debris is generated, and there is no damage to the parts. DETAILED DESCRIPTION

[0047] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] The following table shows the purchase channels of the chemical reagents used in the present invention:

[0049] Reagent name Purity Grade Manufacturer Deionized water Industrial Grade Suzhou Ein Water Treatment Company Ether Industrial Grade Jiangsu Qiangsheng Functional Chemistry 2-Aminoethyl methacrylate Analytical grade Zhende Chemical Potassium carbonate Chemically pure Jiangsu Qiangsheng Functional Chemistry Benzyl chloroformate Analytical grade Jiangsu Qiangsheng Functional Chemistry Glycine Analytical grade Jiangsu Qiangsheng Functional Chemistry Ammonium chloride Chemically pure Jiangsu Qiangsheng Functional Chemistry 4-tert-Butylcyclohexyl acrylate Analytical grade Changxing Chemical Isotridecyl methacrylate Analytical grade Changxing Chemical Benzoyl peroxide Analytical grade Aladdin Chemistry Azobisisobutyronitrile Analytical grade Aladdin Chemistry Toluene Industrial Grade Suzhou Chengxiang Chemical Xylene Industrial Grade Suzhou Chengxiang Chemical Ethyl acetate Industrial Grade Suzhou Chengxiang Chemical 33% Hydrogen bromide acetic acid solution Analytical grade Aladdin Chemistry Black color paste Industrial Grade Zhongfucai JQ1908 Stearic acid methacrylate Analytical grade Changxing Chemical 2-Aminoethyl acrylate Analytical grade Zhende Chemical Sodium carbonate Chemically pure Jiangsu Qiangsheng Functional Chemistry Ethoxyethoxyethyl acrylate Analytical grade Changxing Chemical Polyisocyanate Analytical grade Anzo Chemical Y-105 Epoxy Curing Agent Analytical grade Anzuo Chemical Y-202 Metal salt curing agent Analytical grade Shimei Chemical PX-4100

[0050] Example 1

[0051] S1. Preparation of benzyloxycarbonyl protected aminoacrylic acid monomer:

[0052] Add 375 ml of deionized water, 375 ml of ether, 32.3 g of 2-aminoethyl methacrylate and 190 g of potassium carbonate to a 3000 ml three-necked flask, then cool to 0 ° C and stir for 30 minutes to obtain a mixed solution. Slowly add 42.7 g of benzyl chloroformate to the mixed solution using a separatory funnel within 90 minutes, and stir at room temperature for 4 hours. Add 3.8 g of glycine to remove excess benzyl chloroformate, and stir at room temperature for 20 hours. Wash the organic phase with saturated ammonium chloride solution, deionized water and saturated salt water, respectively, and then wash with anhydrous Na 2 SO 4 The mixture was dried, filtered, concentrated by rotary evaporation, and dried in vacuo to obtain 2-(benzyloxycarbonylamino)ethyl methacrylate.

[0053] S2. Preparation of acrylic polymers containing primary amine groups in side chains;

[0054] 45g of 4-tert-butylcyclohexyl acrylate, 30g of isotridecyl methacrylate, 15g of 2-(benzyloxycarbonylamino)ethyl methacrylate, 0.1g of benzoyl peroxide, 0.3g of azobisisobutyronitrile, 40g of toluene and 90g of ethyl acetate were uniformly mixed to obtain a mixed solution. 2 / 3 of the mixed solution was placed in a constant temperature oil bath at 80°C, and after free radical polymerization for 3h, the remaining mixed solution was slowly dripped and dripped within 2h, and then the constant temperature reaction was continued for 4h. Finally, 31.5g of 33% hydrogen bromide acetic acid solution was added to deprotect the amino group to obtain an acrylic polymer containing primary amine groups in the side chain. The prepared acrylic polymer containing primary amine groups in the side chain has a content ratio of amine groups to acrylic acid solids of 0.63mmol / g, a viscosity of 1800mPa.s / 25°C, a glass transition temperature of -30°C, a weight average molecular weight of 175000, and a molecular weight distribution of 2.2.

[0055] 400 parts of toluene and 3 parts of polyisocyanate were added to 100 parts of acrylic polymer containing primary amine groups in the side chain, and the mixture was stirred for 15 minutes. After the mixture was evenly mixed, 0.5um dry glue was coated on the surface of 500um polyurethane foam by a micro-concave coater, and the mixture was dried at 100°C for 3 minutes. The step was repeated, and 0.5um dry glue was coated on the other side of the foam to obtain a polyurethane foam substrate with acrylic polymer coatings on both sides.

[0056] S3. Preparation of a low temperature heavy duty foam tape

[0057] a. Mix 100 parts of acrylic pressure-sensitive adhesive, 7 parts of tackifying resin, 3 parts of black color paste, 0.6 parts of curing agent and 90 parts of solvent by weight, and perform ultrasonic dispersion to obtain a pressure-sensitive adhesive;

[0058] Acrylic pressure-sensitive adhesive, Y-1421 from Anzu Chemical, has a glass transition temperature of -12°C, a weight average molecular weight of 800,000, and a molecular weight distribution of 1.7; the storage modulus at -40°C is 420,000 KPa, and the loss factor is 0.075; the storage modulus at 23°C is 160 KPa, and the loss factor is 1.08; the storage modulus of the acrylic pressure-sensitive adhesive at 85°C is 35 KPa, and the loss factor is 0.29;

[0059] The tackifying resin is a terpene phenol resin with a softening point of 150°C, specifically TP1150 from Kraton; the curing agent is a polyisocyanate and an epoxy curing agent, with a mass ratio of 1:1; the solvent is ethyl acetate;

[0060] b. Coat a 50 μm thick pressure-sensitive adhesive on the release surface of a 50 μm thick release film having an aged release force of 42 gf / in, a 24h release force of 35 gf / in, and a residual rate of 85%, and dry at 110° C. for 5 min to obtain a pressure-sensitive adhesive layer A;

[0061] c. Coat a 50 μm thick pressure-sensitive adhesive on the release surface of a 50 μm thick release film with an aged release force of 20 gf / in, a 24h release force of 15 gf / in, and a residual rate of 86%, and dry at 110°C for 5 minutes to obtain a pressure-sensitive adhesive layer B; laminate the pressure-sensitive adhesive layer A on a foam substrate to obtain a semi-finished product; laminate the pressure-sensitive adhesive layer B on the other side of the semi-finished product to obtain a low-temperature reworked foam tape; the thickness of the pressure-sensitive adhesive layer A and the pressure-sensitive adhesive layer B is 50 μm.

[0062] Example 2

[0063] S1. Preparation of benzyloxycarbonyl protected aminoacrylic acid monomer;

[0064] Add 375 ml of deionized water, 375 ml of ether, 32.3 g of 2-aminoethyl methacrylate and 190 g of potassium carbonate to a 3000 ml three-necked flask, then cool to 0 °C and stir for 30 min. Add 42.7 g of benzyl chloroformate slowly to the mixed solution using a separatory funnel over 90 min, and stir at room temperature for 4 h. Add 3.8 g of glycine to remove excess benzyl chloroformate, and stir at room temperature for 20 h. Wash the organic phase with saturated ammonium chloride solution, deionized water and saturated saline, and then rinse with anhydrous Na 2 SO 4 The mixture was dried, filtered, concentrated by rotary evaporation, and dried in vacuo to obtain 2-(benzyloxycarbonylamino)ethyl methacrylate.

[0065] S2. Preparation of acrylic polymers containing primary amine groups in side chains;

[0066] 55g of 4-tert-butylcyclohexyl acrylate, 30g of stearic acid methacrylate, 20g of 2-(benzyloxycarbonylamino)ethyl methacrylate, 0.15g of benzoyl peroxide, 0.2g of azobisisobutyronitrile, 40g of toluene and 90g of ethyl acetate were uniformly mixed to obtain a mixed solution. 2 / 3 of the mixed solution was added to a 2000mL four-necked flask with a mechanical stirrer, a condenser and a constant pressure titration funnel, and then placed in a constant temperature oil bath at a temperature of 85°C. After free radical polymerization for 2h, the remaining mixed solution was slowly dripped and dripped within 2h, and then the reaction was continued at a constant temperature for 4h. Finally, 41.9g of 33% hydrogen bromide acetic acid solution was added to deprotect the amino group to obtain an acrylic polymer containing primary amine groups in the side chain. The prepared side chain contains primary amine acrylic polymer, the content ratio of amine to acrylic solid is 0.72mmol / g, the viscosity is 1900mPa·s / 25℃, the glass transition temperature is -32℃, the weight average molecular weight is 155000, and the molecular weight distribution is 2.8.

[0067] 300 parts of xylene and 1 part of epoxy curing agent were added to 100 parts of acrylic polymer containing primary amine groups in the side chain, and the mixture was stirred for 15 minutes. After the mixture was evenly mixed, 0.7um dry glue was coated on the surface of 800um polyurethane foam by a micro-concave coater, and the mixture was dried at 110°C for 5 minutes. The step was repeated, and 0.7um dry glue was coated on the other side of the foam to obtain a polyurethane foam substrate with acrylic polymer coatings on both sides.

[0068] S3. Preparation of a low temperature heavy duty foam tape

[0069] a. Mix 100 parts of acrylic pressure-sensitive adhesive, 20 parts of tackifying resin, 4 parts of black color paste, 0.6 parts of curing agent and 110 parts of solvent by mass, stir and ultrasonically disperse to obtain a pressure-sensitive adhesive;

[0070] Acrylic pressure-sensitive adhesive, specifically PS8281F from Shimei Chemical, has a glass transition temperature of -13°C, a weight average molecular weight of 450,000, and a molecular weight distribution of 1.8; a storage modulus of 420,000 KPa at -40°C, and a loss factor of 0.073; a storage modulus of 120 KPa at 23°C, and a loss factor of 1.19; the storage modulus of the acrylic pressure-sensitive adhesive at 85°C is 15 KPa, and the loss factor is 0.56;

[0071] The tackifying resin is a rosin resin with a softening point of 150°C, specifically T803L produced by Arakawa Chemical; the curing agent is a polyisocyanate and an epoxy curing agent, with a mass ratio of 1 / 1.2; the solvent is ethyl acetate;

[0072] b. Coat a 50 μm thick pressure-sensitive adhesive on the release surface of a 50 μm thick release film having an aged release force of 40 gf / in, a 24h release force of 37 gf / in, and a residual rate of 86%, and dry at 110° C. for 5 minutes to obtain a pressure-sensitive adhesive layer A;

[0073] c. Coat a pressure-sensitive adhesive with a thickness of 50 μm on the release surface of a release film with an aged release force of 18 gf / in, a 24h release force of 12 gf / in, and a residual rate of 83%, and dry at 110°C for 5 minutes to obtain a pressure-sensitive adhesive layer B; laminate the pressure-sensitive adhesive layer A on a foam substrate to obtain a semi-finished product; laminate the pressure-sensitive adhesive layer B on the other side of the semi-finished product to obtain a low-temperature reworked foam tape; the thickness of the pressure-sensitive adhesive layer A and the pressure-sensitive adhesive layer B is 50 μm.

[0074] Example 3

[0075] S1. Preparation of benzyloxycarbonyl protected aminoacrylic acid monomer;

[0076] Add 400ml of deionized water, 400ml of ether, 32.3g of 2-aminoethyl acrylate and 159g of sodium carbonate to a 3000ml three-necked flask, then cool to 0°C and stir for 30min. Slowly add 51.2g of benzyl chloroformate to the mixed solution using a separatory funnel within 90min, then remove the ice-water bath and stir at room temperature for 4h. Add 3.8g of glycine to remove excess benzyl chloroformate and stir at room temperature for 20h. Wash the organic phase with saturated ammonium chloride solution, deionized water and saturated saline, and then rinse with anhydrous Na 2 SO4 drying, suction filtration, rotary evaporation concentration of the filtrate, and vacuum drying to obtain 2-(benzyloxycarbonylamino)ethyl acrylate.

[0077] S2. Preparation of acrylic polymers containing primary amine groups in side chains;

[0078] 40g of ethoxyethoxyethyl acrylate, 35g of stearic acid methacrylate, 18g of 2-(benzyloxycarbonylamino)ethyl acrylate, 0.35g of azobisisobutyronitrile, 45g of toluene and 95g of ethyl acetate were uniformly mixed to obtain a mixed solution. 2 / 3 of the mixed solution was added to a 2000mL four-necked flask with a mechanical stirrer, a condenser and a constant pressure titration funnel, and then placed in a constant temperature oil bath at 90°C. After free radical polymerization for 1.5h, the remaining mixed solution was slowly dripped and dripped within 2h, and then the reaction was continued at a constant temperature for 4h. Finally, 39.6g of 33% hydrogen bromide acetic acid solution was added to deprotect the amino group to obtain an acrylic polymer containing primary amine groups in the side chain. The prepared acrylic polymer has primary amine groups in the side chain, the content ratio of amine groups to acrylic acid solids is 0.78 mmol / g, the viscosity is 1600 mPa·s / 25°C, the glass transition temperature is -35°C, the weight average molecular weight is 125000, and the molecular weight distribution is 3.0.

[0079] 500 parts of toluene and 5 parts of metal salt curing agent were added to 100 parts of acrylic polymer containing primary amine groups in the side chain, and the mixture was stirred for 15 minutes. After the mixture was evenly mixed, 0.5 um dry glue was coated on the surface of 700 um polyethylene foam by a micro-concave coater, and the mixture was dried at 100°C for 3 minutes. The step was repeated, and 0.5 um dry glue was coated on the other side of the foam to obtain a polyurethane foam substrate with acrylic polymer coatings on both sides.

[0080] S3. Preparation of a low temperature heavy duty foam tape

[0081] a. Mix 100 parts of acrylic pressure-sensitive adhesive, 25 parts of tackifying resin, 3 parts of black color paste, 0.8 parts of curing agent and 125 parts of solvent by mass, stir and ultrasonically disperse to obtain a pressure-sensitive adhesive;

[0082] Acrylic pressure-sensitive adhesive, specifically Y-1510 from Anzu Chemical, has a glass transition temperature of -10°C, a weight average molecular weight of 750,000, and a molecular weight distribution of 1.8; a storage modulus of 671,000 KPa at -40°C, and a loss factor of 0.087; a storage modulus of 103 KPa at 23°C, and a loss factor of 0.96; the storage modulus of the acrylic pressure-sensitive adhesive at 85°C is 18 KPa, and the loss factor is 0.40;

[0083] The tackifying resin is a rosin resin with a softening point of 110°C, specifically Kraton's RE110L; the curing agent is a polyisocyanate and an epoxy curing agent, with a mass ratio of 1 / 1.5; the solvent is toluene;

[0084] b. Coat a 50 μm thick pressure-sensitive adhesive on the release surface of a release film having an aging release force of 48 gf / in, a 24h release force of 40 gf / in, and a residual rate of 83% and dry at 110° C. for 5 min to obtain a pressure-sensitive adhesive layer A;

[0085] c. Coat a pressure-sensitive adhesive with a thickness of 50 μm on the release surface of a release film with an aged release force of 25 gf / in, a 24h release force of 15 gf / in, and a residual rate of 84%, and dry at 110°C for 5 minutes to obtain a pressure-sensitive adhesive layer B; laminate the pressure-sensitive adhesive layer A on a foam substrate to obtain a semi-finished product; laminate the pressure-sensitive adhesive layer B on the other side of the semi-finished product to obtain a low-temperature reworked foam tape; the thickness of the pressure-sensitive adhesive layer A and the pressure-sensitive adhesive layer B is 40 μm.

[0086] Comparative Example 1

[0087] Example 1 was used as a control group, but no acrylic polymer containing primary amine groups in the side chains was coated on the foam surface;

[0088] a. Mix 100 parts of acrylic pressure-sensitive adhesive, 7 parts of tackifying resin, 3 parts of black color paste, 0.6 parts of curing agent and 90 parts of solvent by weight, and perform ultrasonic dispersion to obtain a pressure-sensitive adhesive;

[0089] Acrylic pressure-sensitive adhesive, Y-1421 from Anzu Chemical, has a glass transition temperature of -12°C, a weight average molecular weight of 800,000, and a molecular weight distribution of 1.7; the storage modulus at -40°C is 420,000 KPa, and the loss factor is 0.075; the storage modulus at 23°C is 160 KPa, and the loss factor is 1.08; the storage modulus of the acrylic pressure-sensitive adhesive at 85°C is 35 KPa, and the loss factor is 0.29;

[0090] The tackifying resin is a terpene phenol resin with a softening point of 150°C, specifically TP1150 from Kraton; the curing agent is a polyisocyanate and an epoxy curing agent, with a mass ratio of 1 / 1; the solvent is ethyl acetate;

[0091] b. Coat a 50 μm thick pressure-sensitive adhesive on the release surface of a 50 μm thick release film having an aged release force of 42 gf / in, a 24h release force of 35 gf / in, and a residual rate of 85%, and dry at 110° C. for 5 min to obtain a pressure-sensitive adhesive layer A;

[0092] c. Coat a pressure-sensitive adhesive with a thickness of 50 μm on the release surface of a release film with an aged release force of 20 gf / in, a 24h release force of 15 gf / in, and a residual rate of 86%, and dry at 110°C for 5 minutes to obtain a pressure-sensitive adhesive layer B; laminate the pressure-sensitive adhesive layer A on a foam substrate to obtain a semi-finished product; laminate the pressure-sensitive adhesive layer B on the other side of the semi-finished product to obtain a low-temperature reworked foam tape; the thickness of the pressure-sensitive adhesive layer A and the pressure-sensitive adhesive layer B is 50 μm.

[0093] Comparative Example 2

[0094] Using Example 2 as a control group, the content ratio of the acrylic polymer amine group containing a primary amine group in the side chain and the acrylic solid, the viscosity, the glass transition temperature, the weight average molecular weight, and the molecular weight distribution were changed;

[0095] S 1. Preparation of benzyloxycarbonyl protected aminoacrylic acid monomer;

[0096] Add 375 ml of deionized water, 375 ml of ether, 32.3 g of 2-aminoethyl methacrylate and 190 g of potassium carbonate to a 3000 ml three-necked flask, then cool to 0 °C and stir for 30 min. Add 42.7 g of benzyl chloroformate slowly to the mixed solution using a separatory funnel over 90 min, and stir at room temperature for 4 h. Add 3.8 g of glycine to remove excess benzyl chloroformate, and stir at room temperature for 20 h. Wash the organic phase with saturated ammonium chloride solution, deionized water and saturated saline, and then rinse with anhydrous Na 2 SO 4 The mixture was dried, filtered, concentrated by rotary evaporation, and dried in vacuo to obtain 2-(benzyloxycarbonylamino)ethyl methacrylate.

[0097] S2. Preparation of acrylic polymers containing primary amine groups in side chains;

[0098] 50g of 4-tert-butylcyclohexyl acrylate, 50g of stearic acid methacrylate, 5g of 2-(benzyloxycarbonylamino)ethyl methacrylate, 0.15g of benzoyl peroxide, 0.2g of azobisisobutyronitrile, 40g of toluene and 90g of ethyl acetate were uniformly mixed to obtain a mixed solution. 2 / 3 of the mixed solution was added to a 2000mL four-necked flask with a mechanical stirrer, a condenser and a constant pressure titration funnel, and then placed in a constant temperature oil bath pot at a temperature of 85°C. After free radical polymerization for 2h, the remaining mixed solution was slowly dripped and dripped within 2h, and then the reaction was continued at a constant temperature for 4h. Finally, 41.9g of 33% hydrogen bromide acetic acid solution was added to deprotect the amino group to obtain an acrylic polymer containing primary amine groups in the side chain. The prepared acrylic polymer has primary amine groups in the side chain, the content ratio of amine groups to acrylic acid solids is 0.19 mmol / g, the viscosity is 2300 mPa·s / 25°C, the glass transition temperature is -50°C, the weight average molecular weight is 255000, and the molecular weight distribution is 3.8.

[0099] 300 parts of xylene and 1 part of epoxy curing agent were added to 100 parts of acrylic polymer containing primary amine groups in the side chain, and the mixture was stirred for 15 minutes. After the mixture was evenly mixed, 0.7um dry glue was coated on the surface of 800um polyurethane foam by a micro-concave coater, and the mixture was dried at 100°C for 3 minutes. The step was repeated, and 0.7um dry glue was coated on the other side of the foam to obtain a polyurethane foam substrate with acrylic polymer coatings on both sides.

[0100] S3. Preparation of a low temperature heavy duty foam tape

[0101] a. Mix 100 parts of acrylic pressure-sensitive adhesive, 20 parts of tackifying resin, 4 parts of black color paste, 0.6 parts of curing agent and 110 parts of solvent by mass, stir and ultrasonically disperse to obtain a pressure-sensitive adhesive;

[0102] Acrylic pressure-sensitive adhesive, specifically PS8281F from Shimei Chemical, has a glass transition temperature of -13°C, a weight average molecular weight of 450,000, and a molecular weight distribution of 1.8; a storage modulus of 420,000 KPa at -40°C, and a loss factor of 0.073; a storage modulus of 120 KPa at 23°C, and a loss factor of 1.19; the storage modulus of the acrylic pressure-sensitive adhesive at 85°C is 15 KPa, and the loss factor is 0.56;

[0103] The tackifying resin is a rosin resin with a softening point of 150°C, specifically T803L produced by Arakawa Chemical; the curing agent is a polyisocyanate and an epoxy curing agent, with a mass ratio of 1 / 1.2; the solvent is ethyl acetate;

[0104] b. Coat a 50 μm thick pressure-sensitive adhesive on the release surface of a 50 μm thick release film having an aged release force of 40 gf / in, a 24h release force of 37 gf / in, and a residual rate of 86%, and dry at 110° C. for 5 minutes to obtain a pressure-sensitive adhesive layer A;

[0105] c. Coat a pressure-sensitive adhesive with a thickness of 50 μm on the release surface of a release film with an aged release force of 18 gf / in, a 24h release force of 12 gf / in, and a residual rate of 83%, and dry at 110°C for 5 minutes to obtain a pressure-sensitive adhesive layer B; laminate the pressure-sensitive adhesive layer A on a foam substrate to obtain a semi-finished product; laminate the pressure-sensitive adhesive layer B on the other side of the semi-finished product to obtain a low-temperature reworked foam tape; the thickness of the pressure-sensitive adhesive layer A and the pressure-sensitive adhesive layer B is 50 μm.

[0106] Comparative Example 3

[0107] Using Example 3 as a control group, the glass transition temperature of the acrylic pressure-sensitive adhesive was changed; the storage modulus and loss factor at -40°C; and the storage modulus and loss factor at 23°C.

[0108] s1. Preparation of benzyloxycarbonyl protected aminoacrylic acid monomer;

[0109] Add 400ml of deionized water, 400ml of ether, 32.3g of 2-aminoethyl acrylate and 159g of sodium carbonate to a 3000ml three-necked flask, then cool to 0°C and stir for 30min. Slowly add 51.2g of benzyl chloroformate to the mixed solution using a separatory funnel within 90min, then remove the ice-water bath and stir at room temperature for 4h. Add 3.8g of glycine to remove excess benzyl chloroformate and stir at room temperature for 20h. Then, wash the organic phase with saturated ammonium chloride solution, deionized water and saturated saline, and then wash with anhydrous Na 2 SO 4 The mixture was dried, filtered, concentrated by rotary evaporation, and dried in vacuo to obtain 2-(benzyloxycarbonylamino)ethyl acrylate.

[0110] S2. Preparation of acrylic polymers containing primary amine groups in side chains;

[0111] 40g of ethoxyethoxyethyl acrylate, 35g of stearic acid methacrylate, 18g of 2-(benzyloxycarbonylamino)ethyl acrylate, 0.35g of azobisisobutyronitrile, 45g of toluene and 95g of ethyl acetate were uniformly mixed to obtain a mixed solution. 2 / 3 of the mixed solution was added to a 2000mL four-necked flask with a mechanical stirrer, a condenser and a constant pressure titration funnel, and then placed in a constant temperature oil bath at 90°C. After free radical polymerization for 1.5h, the remaining mixed solution was slowly dripped and dripped within 2h, and then the reaction was continued at a constant temperature for 4h. Finally, 39.6g of 33% hydrogen bromide acetic acid solution was added to deprotect the amino group to obtain an acrylic polymer containing primary amine groups in the side chain. The prepared acrylic polymer has primary amine groups in the side chain, the content ratio of amine groups to acrylic acid solids is 0.78 mmol / g, the viscosity is 1600 mPa·s / 25°C, the glass transition temperature is -35°C, the weight average molecular weight is 125000, and the molecular weight distribution is 3.0.

[0112] 500 parts of toluene and 5 parts of metal salt curing agent were added to 100 parts of acrylic polymer containing primary amine groups in the side chain. After mixing evenly, 0.5um dry glue was coated on the surface of 700um polyethylene foam by a micro-concave coater, and dried at 100°C for 3 minutes. This step was repeated, and 0.5um dry glue was coated on the other side of the foam to obtain a polyurethane foam substrate with acrylic polymer coatings on both sides.

[0113] S3. Preparation of a low temperature heavy duty foam tape

[0114] a. Mix 100 parts of acrylic pressure-sensitive adhesive, 25 parts of tackifying resin, 3 parts of black color paste, 0.8 parts of curing agent and 125 parts of solvent by mass, stir and ultrasonically disperse to obtain a pressure-sensitive adhesive;

[0115] The acrylic pressure-sensitive adhesive, specifically Y-1423 from Anzo Chemical, has a glass transition temperature of -25°C, a weight average molecular weight of 550,000, and a molecular weight distribution of 1.89; the storage modulus at -40°C is 310,000 KPa, and the loss factor is 0.23; the storage modulus at 23°C is 74 KPa, and the loss factor is 0.62; the storage modulus of the acrylic pressure-sensitive adhesive at 85°C is 23 KPa, and the loss factor is 0.35.

[0116] The tackifying resin is a rosin resin with a softening point of 110°C, specifically Kraton's RE110L; the curing agent is a polyisocyanate and an epoxy curing agent, with a mass ratio of 1 / 1.5; the solvent is toluene;

[0117] b. Coat a 50 μm thick pressure-sensitive adhesive on the release surface of a release film having an aging release force of 48 gf / in, a 24h release force of 40 gf / in, and a residual rate of 83% and dry at 110° C. for 5 min to obtain a pressure-sensitive adhesive layer A;

[0118] c. Coat a 50 μm thick pressure-sensitive adhesive on the release surface of a 50 μm thick release film with an aged release force of 25 gl / in, a 24h release force of 15 gf / in, and a residual rate of 84%, and dry at 110°C for 5 minutes to obtain a pressure-sensitive adhesive layer B; laminate the pressure-sensitive adhesive layer A on a foam substrate to obtain a semi-finished product; laminate the pressure-sensitive adhesive layer B on the other side of the semi-finished product to obtain a low-temperature reworked foam tape; the thickness of the pressure-sensitive adhesive layer A and the pressure-sensitive adhesive layer B is 40 μm.

[0119] experiment

[0120] The normal temperature and high temperature and high humidity peel strength, rolling ball initial adhesion, high temperature and high humidity retention, and low temperature reworkability of the adhesive tapes prepared in Examples 1-3 and Comparative Examples 1-3 were tested, and the test results are shown in the following table;

[0121] The peel strength of the prepared tape was measured with reference to the method of GB / T2792-2014: the adhered object was a steel plate SUS with a bright surface and a roughness of 50nm (GB / T2523-2008). The tape was cut into a size of 25mm×300mm, and pressed back and forth 3 times with a 2kg roller, and left for 20min. The test environment was 23℃ / 50%RH at room temperature, and 80℃ / 90%RH at high temperature and high humidity. The tape was peeled 180° at a speed of 300mm / min.

[0122] The rolling ball initial adhesion of the prepared tape was measured with reference to the method of JIS Z0237: the J.DOW method was adopted: on a smooth surface with an inclination of 30°, a rolling ball with a diameter of 2 / 32 inch to 32 / 32 inch was used to slide down from the starting point of the sliding distance, and the maximum rolling ball number of the steel ball on the rubber surface was measured; the test environment was 23℃ / 65%RH, the sliding distance was 100mm; the sliding distance was 100mm; the test instrument was a tape initial adhesion rolling ball tester;

[0123] High temperature and high humidity retention: Wipe the retention test plate SUS with anhydrous ethanol and a dust-free cloth, and dry it naturally at room temperature for more than 5 minutes; reinforce the non-test surface of the tape with 25μm PET, cut it into 25mm×100mm strips, and stick it on the test plate SUS with an area of ​​25mm×20mm. The remaining length is used to fix the loading plate. A 2Kg roller is manually rolled back and forth 3 times to make it fit with the SUS, and there are no bubbles between the steel plate and the sample; after the sample is prepared and left to stand for 20 minutes, it is hung in the retention tester with high temperature and high humidity. The high temperature and high humidity test environment is 80℃ / 90%RH, and a 1KG weight is added; record the time when the steel plate below falls. If no steel plate falls off, record the distance the strip moves down within 48H; the result is expressed as the time when the steel plate falls off or the distance the strip moves down.

[0124] Low temperature reworkability: Place the prepared tape at 23±1℃ and 50±5%RH for 24h, cut 5mm×10cm strips, and then stick both sides of the tape to the objects, press back and forth with a 2kg roller 3 times, and leave for 24h. Put the parts that need to be reworked or repaired in a -40℃ refrigeration device for 10min, then take out and gently separate the bonded parts, remove the tape from the parts after returning to room temperature, and observe the low temperature reworkability.

[0125] The performance comparison of the adhesive tapes prepared in Examples 1-3 and Comparative Examples 1-3 is shown in the following table:

[0126]

[0127] Conclusion: By comparing the examples with the comparative examples, it can be seen that when the foam tape prepared by the method provided by the present invention is reworked, there is no residual glue or degumming during the entire process of removing the tape from the parts, no foam debris is generated, and there is no damage to the parts.

[0128] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A low temperature heavy duty foam tape, characterized in that: The foam tape comprises a substrate, which is a foam substrate coated with acrylic polymer coatings on both sides, a pressure-sensitive adhesive layer is attached to one side or both sides of the substrate, and a release film is attached to the outer side of the pressure-sensitive adhesive layer; The acrylic polymer coating is mainly composed of an acrylic polymer coating containing primary amine groups in the side chains; The acrylic polymer containing primary amino groups in the side chain is mainly obtained by free radical polymerization of low shrinkage acrylic monomer and benzyloxycarbonyl protected amino acrylic monomer under the action of an initiator; The acrylic polymer containing primary amine groups in the side chain is composed of the following components: by weight, 75-85 parts of low shrinkage acrylic monomer; 15-20 parts of benzyloxycarbonyl protected amino acrylic monomer; 0.1-0.5 parts of thermal initiator; and 80-150 parts of solvent; The low shrinkage acrylic monomer is any one or more of 4-tert-butyl cyclohexyl acrylate, stearic acid methacrylate, lauric acid methacrylate, ethoxyethoxyethyl acrylate, isotridecyl methacrylate, and octadecyl acrylate; the benzyloxycarbonyl protected amino acrylic monomer is any one or more of methacrylate-2-(benzyloxycarbonylamino)ethyl ester and acrylate-2-(benzyloxycarbonylamino)ethyl ester; The side chain of the acrylic polymer contains primary amine groups, the content ratio of amine groups to acrylic acid solids is 0.5-1.5 mmol / g, the viscosity is 500-2000 mPa·s / 25°C, the glass transition temperature is -40-50°C, and the weight average molecular weight is 50000-200000; The pressure-sensitive adhesive layer includes an acrylic pressure-sensitive adhesive, and the acrylic pressure-sensitive adhesive is one of Anzuo Chemical's Y-1421, Anzuo Chemical's Y-1510, and Shimei Chemical's PS8281F.

2. A low temperature heavy duty foam tape according to claim 1, characterized in that: The acrylic polymer coating is composed of the following ingredients: by weight: 100 parts of acrylic polymer containing primary amine groups in the side chains; 1-5 parts of curing agent; 300-500 parts of solvent.

3. A low temperature heavy duty foam tape according to claim 2, characterized in that: The curing agent is any one or more of polyisocyanate, epoxy curing agent and metal salt curing agent.

4. The low temperature heavy duty foam tape according to claim 1, characterized in that: The thermal initiator is any one or more of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, lauroyl peroxide, and tert-butyl perbenzoate.

5. The low temperature heavy duty foam tape according to claim 1, characterized in that: The pressure-sensitive adhesive layer is composed of the following ingredients: by weight: 100 parts of acrylic pressure-sensitive adhesive; 5-30 parts of tackifying resin; 1-5 parts of black color paste; Curing agent 0.2-3 parts; Solvent 50-200 parts.

6. A low temperature heavy duty foam tape according to claim 5, characterized in that: The tackifying resin is any one or more of rosin resin, modified rosin resin, terpene resin and petroleum resin; the curing agent is any one or more of polyisocyanate, epoxy curing agent and metal salt curing agent.

7. The low temperature heavy duty foam tape according to claim 1, characterized in that: The thickness of the substrate is 0.05-3 mm; The thickness of the pressure-sensitive adhesive layer is 5-100 μm; The release film has a thickness of 50-100 μm; The substrate is any one or more of polyurethane foam, polyethylene foam, and polypropylene foam.

8. A method for preparing a low-temperature heavy-duty foam tape, characterized in that: The following steps are included: Step 1: Take a low-shrinkage acrylic monomer, a benzyloxycarbonyl-protected amino acrylic monomer, a thermal initiator, and a solvent, mix them evenly, react at 65-90° C. for 6-10 hours, add a hydrogen bromide acetic acid solution to deprotect the amino group, and obtain an acrylic polymer containing a primary amino group in the side chain; Step 2: Take an acrylic polymer having a primary amine group in the side chain, a curing agent, and a solvent, mix them evenly to obtain an acrylic polymer; apply the acrylic polymer on both sides of the foam substrate, and dry at 90-120° C. for 3-10 minutes to obtain an acrylic polymer coating; Step 3: Mixing and stirring the acrylic pressure-sensitive adhesive, tackifying resin, black color paste, curing agent, and solvent, and ultrasonically dispersing the mixture to obtain a pressure-sensitive adhesive; Step 4: coating a pressure-sensitive adhesive on the release surface of the release film, drying the pressure-sensitive adhesive layer, and laminating the pressure-sensitive adhesive layer on a foam substrate to obtain a low-temperature reworkable foam tape.

9. The method for preparing a low-temperature heavy-duty foam tape according to claim 8, characterized in that: The preparation method of the benzyloxycarbonyl protected aminoacrylic acid monomer comprises: taking deionized water, ether, aminoacrylic acid monomer, and alkaline reagent, stirring evenly, dropping benzyl chloroformate, stirring, adding glycine, stirring and reacting for 19-21 hours, washing, drying, filtering, concentrating the filtrate by rotary evaporation, and vacuum drying to obtain the benzyloxycarbonyl protected aminoacrylic acid monomer; The aminoacrylic acid monomer is any one or more of 2-aminoethyl methacrylate and 2-aminoethyl acrylate; the alkaline reagent is any one or more of sodium carbonate, potassium carbonate, sodium bicarbonate and sodium hydroxide.